Home » Precipitation Hardened Stainless Steels » 17-4PH Cast H1000 Stainless Steel Material Data Sheet
17-4PH Cast H1000 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
17-4PH Cast H1000 Overview
17-4PH cast H1000 is a martensitic precipitation hardening stainless steel (UNS S17400) in the cast form. Condition: H1000 – Solution treated and precipitation/age hardened at 1000°F (538°C). This 17-4PH cast H1000 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-4PH castings from Turkey (Türkiye)? Modulus Metal supplies 17-4PH castings with in-house CNC machining and inspects them before shipment.
17-4PH Designation
17-4PH Condition H1000 – Solution treated and precipitation/age hardened at 1000°F (538°C) UNS number S17400 US name ASTM S17400, ASTM 61, AMS 5355 GB (Chinese) name 0Cr17Ni4Cu4Nb, 0Cr16Ni4Cu4Nb JIS (Japanese) name SUSF630, SUS630 Tradenames 17-4 PH, AK Steel (USA); 17-4PH, Sandmeyer (USA); CATAMOLD 17-4PH, BASF (USA); AMS 5643 – 17/4 PH, Smiths (UK);
17-4PH Cast H1000 Composition detail
Al (aluminum) 0 – 0.05 % C (carbon) 0 – 0.06 % Cr (chromium) 15.5 – 16.7 % Cu (copper) 2.8 – 3.5 % Fe (iron) 72.8 – 77.4 % Mn (manganese) 0 – 0.7 % N (nitrogen) 0 – 0.05 % Nb (niobium) 0.15 – 0.4 % Ni (nickel) 3.6 – 4.6 % P (phosphorus) 0 – 0.025 % S (sulfur) 0 – 0.025 % Si (silicon) 0.5 – 1 % Sn (tin) 0 – 0.02 % Ta (tantalum) 0 – 0.05 %
17-4PH Physical properties
17-4PH Cast H1000 Mechanical properties
Young’s modulus 197 – 207 GPa Specific stiffness 25.1 – 26.5 MN.m/kg Yield strength (elastic limit) 896 – 990 MPa Tensile strength 1030 – 1140 MPa Specific strength 114 – 126 kN.m/kg Elongation 4 – 4.65 % strain Compressive strength 910 – 1010 MPa Flexural modulus 197 – 207 GPa Flexural strength (modulus of rupture) 896 – 990 MPa Shear modulus 88 – 92.5 GPa Bulk modulus 142 – 150 GPa Poisson’s ratio 0.27 – 0.281 Shape factor 25 Hardness – Vickers 250 – 460 HV Elastic stored energy (springs) 1990 – 2430 kJ/m3 Fatigue strength at 10^7 cycles 364 – 542 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 357 – 552 MPa
17-4PH Impact & fracture properties
Fracture toughness 116 – 142 MPa.m0.5 Toughness (G) 67.3 – 98.9 kJ/m2
17-4PH Cast H1000 Thermal properties
Melting point 1400 – 1440 °C Maximum service temperature 282 – 316 °C Minimum service temperature -73 – -43 °C Thermal conductivity 17.3 – 18.7 W/m.°C Specific heat capacity 477 – 496 J/kg.°C Thermal expansion coefficient 12.5 – 13.1 µstrain/°C Thermal shock resistance 342 – 387 °C Thermal distortion resistance 1.34 – 1.47 MW/m Latent heat of fusion 260 – 285 kJ/kg
17-4PH Electrical properties
Electrical resistivity 75 – 85 µohm.cm Electrical conductivity 2.03 – 2.3 %IACS Galvanic potential -0.2 – -0.12 V
17-4PH Magnetic properties
17-4PH Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 5010 – 5140 m/s Mechanical loss coefficient (tan delta) 3.1e-4 – 6.6e-4
17-4PH Processing properties
Metal casting Limited use Metal cold forming Unsuitable Metal hot forming Unsuitable Metal press forming Unsuitable Metal deep drawing Unsuitable Machining speed 13.1 m/min Weldability Notes: Preheating is not required, post weld heat treatment is required Good Carbon equivalency 0.687 – 0.867
17-4PH Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Excellent Strong acids Acceptable Weak alkalis Excellent Strong alkalis Limited use Organic solvents Excellent Oxidation at 500C Excellent UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. Acceptable Flammability Non-flammable
17-4PH Cast H1000 Corrosion resistance
Pitting resistance equivalent number (PREN) 15.5 – 17.5 Pitting and crevice corrosion Low (<20) Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide Slightly susceptible
17-4PH Standards with similar compositions
USA: 5342 to AMS 5342D, UNS J92150, UNS J92200Tradenames: COOPER 17-4 PH, CORROSALLOY HT, ISO-CAST CB7CU, T-17-4PH, ZCR 173