AISI 1050 Annealed vs As Rolled vs Normalized vs Oil vs Water Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1050 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1050 medium carbon steel (UNS G10500) side by side for 12 conditions: annealed, as rolled, normalized, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C, water quenched & tempered at 205°C, water quenched & tempered at 315°C, water quenched & tempered at 425°C, water quenched & tempered at 540°C, water quenched & tempered at 650°C. All values are taken from the individual AISI 1050 material data sheets linked below.

AISI 1050 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed325–405570–705173–21318–2926.8
As Rolled370–455650–800210–26016–2422.3
Normalized380–475670–825200–24516–2422.9
Oil Quenched & Tempered at 315°C645–800880–1080290–36011–1715.8
Oil Quenched & Tempered at 425°C585–720840–1040250–31016–2417.7
Oil Quenched & Tempered at 540°C520–640785–970240–29018–2818.9
Oil Quenched & Tempered at 650°C420–520660–815205–25023–3522.6
Water Quenched & Tempered at 205°C725–8901010–1240465–5657–1111
Water Quenched & Tempered at 315°C710–875980–1200400–49010–1612.2
Water Quenched & Tempered at 425°C680–835900–1100340–42015–2314
Water Quenched & Tempered at 540°C590–720770–950265–32519–2717.7
Water Quenched & Tempered at 650°C480–595640–795215–26523–3321.9

AISI 1050 Differences Compared with Annealed

The table below shows how much each AISI 1050 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+13%+14%+22%-15%
Normalized+17%+17%+15%-15%
Oil Quenched & Tempered at 315°C+98%+54%+68%-40%
Oil Quenched & Tempered at 425°C+79%+47%+45%-15%
Oil Quenched & Tempered at 540°C+59%+38%+37%-2%
Oil Quenched & Tempered at 650°C+29%+16%+18%+23%
Water Quenched & Tempered at 205°C+121%+76%+167%-62%
Water Quenched & Tempered at 315°C+117%+71%+131%-45%
Water Quenched & Tempered at 425°C+108%+57%+97%-19%
Water Quenched & Tempered at 540°C+79%+35%+53%-2%
Water Quenched & Tempered at 650°C+47%+13%+24%+19%

AISI 1050 Oil Quenched vs Water Quenched

Water removes heat faster than oil, so water quenched AISI 1050 forms more martensite and comes out harder and stronger, but with a higher risk of distortion and quench cracking. The table compares AISI 1050 oil quenched and water quenched material tempered at the same temperature, and shows the difference of water quenching relative to oil quenching (mid-points).

Tempered atYield oil / water (MPa)Yield diff.Tensile oil / water (MPa)Tensile diff.Hardness oil / water (HV)Hardness diff.
315°C645–800 / 710–875+10%880–1080 / 980–1200+11%290–360 / 400–490+37%
425°C585–720 / 680–835+16%840–1040 / 900–1100+6%250–310 / 340–420+36%
540°C520–640 / 590–720+13%785–970 / 770–950-2%240–290 / 265–325+11%
650°C420–520 / 480–595+14%660–815 / 640–795-3%205–250 / 215–265+5%

AISI 1050 Strength and Hardness Charts

Oil quenched & tempered   Water quenched & tempered. Dark bar = minimum, light bar = maximum of the range.

AISI 1050 Yield strength by condition (MPa)Annealed325–405As Rolled370–455Normalized380–475WQ&T 205°C725–890OQ&T 315°C645–800WQ&T 315°C710–875OQ&T 425°C585–720WQ&T 425°C680–835OQ&T 540°C520–640WQ&T 540°C590–720OQ&T 650°C420–520WQ&T 650°C480–595
AISI 1050 Tensile strength by condition (MPa)Annealed570–705As Rolled650–800Normalized670–825WQ&T 205°C1010–1240OQ&T 315°C880–1080WQ&T 315°C980–1200OQ&T 425°C840–1040WQ&T 425°C900–1100OQ&T 540°C785–970WQ&T 540°C770–950OQ&T 650°C660–815WQ&T 650°C640–795
AISI 1050 Hardness by condition (HV)Annealed173–213As Rolled210–260Normalized200–245WQ&T 205°C465–565OQ&T 315°C290–360WQ&T 315°C400–490OQ&T 425°C250–310WQ&T 425°C340–420OQ&T 540°C240–290WQ&T 540°C265–325OQ&T 650°C205–250WQ&T 650°C215–265

AISI 1050 Heat Treatment Key Points

The highest tensile strength of AISI 1050 in these data sheets is reached in the water quenched & tempered at 205°C condition (1010–1240 MPa). The softest condition is annealed (173–213 HV), with a machining speed of 26.8 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1050, raising the tempering temperature from 315°C to 650°C lowers hardness from 290–360 HV to 205–250 HV, trading strength for toughness and ductility. For water quenched AISI 1050, raising the tempering temperature from 205°C to 650°C lowers hardness from 465–565 HV to 215–265 HV, trading strength for toughness and ductility.

AISI 1050 Material Data Sheets

AISI 1050 Annealed | AISI 1050 As Rolled | AISI 1050 Normalized | AISI 1050 Oil Quenched & Tempered at 315°C | AISI 1050 Oil Quenched & Tempered at 425°C | AISI 1050 Oil Quenched & Tempered at 540°C | AISI 1050 Oil Quenched & Tempered at 650°C | AISI 1050 Water Quenched & Tempered at 205°C | AISI 1050 Water Quenched & Tempered at 315°C | AISI 1050 Water Quenched & Tempered at 425°C | AISI 1050 Water Quenched & Tempered at 540°C | AISI 1050 Water Quenched & Tempered at 650°C | All AISI 1050 conditions

Looking for AISI 1050 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1050 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.