PH 13-8Mo H1150 Stainless Steel Material Data Sheet

PH 13-8Mo H1150 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

PH 13-8Mo H1150 Stainless Steel Overview

PH 13-8Mo H1150 stainless steel is a martensitic precipitation hardening stainless steel (UNS S13800) in the wrought form. Condition: H1150 (Solution annealed; precipitation (age) hardened at 621°C; air cooled). This PH 13-8Mo H1150 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for PH 13-8Mo parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PH 13-8Mo parts in-house and inspects them before shipment.

PH 13-8Mo Designation

Korloy 2573, wrought
ConditionH1150 (Solution annealed; precipitation (age) hardened at 621°C; air cooled)
UNS numberS13800
US namePH 13-8Mo
EN nameX3CrNiMoAl13-8-2
EN number1.4534

PH 13-8Mo Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

PH 13-8Mo H1150 Stainless Steel Composition detail

Al (aluminum)0.9–1.35%
C (carbon)0–0.05%
Cr (chromium)12.2–13.2%
Fe (iron)74.1–77.4%
Mn (manganese)0–0.2%
Mo (molybdenum)2–2.5%
N (nitrogen)0–0.01%
Ni (nickel)7.5–8.5%
P (phosphorus)0–0.01%
S (sulfur)0–0.008%
Si (silicon)0–0.1%

PH 13-8Mo Physical properties

Density7.68–7.76g/cm3

PH 13-8Mo H1150 Stainless Steel Mechanical properties

Young’s modulus195–205GPa
Specific stiffness25.2–26.6MN.m/kg
Yield strength (elastic limit)621–686MPa
Tensile strength931–1030MPa
Specific strength80.4–88.9kN.m/kg
Elongation18.5–21.5% strain
Compressive strength1380–1520MPa
Flexural modulus195–205GPa
Flexural strength (modulus of rupture)621–686MPa
Shear modulus76–79.9GPa
Bulk modulus148–155GPa
Poisson’s ratio0.28–0.291 
Shape factor37
Hardness – Vickers400–480HV
Hardness – Rockwell B105–109HRB
Hardness – Rockwell C30–35HRC
Hardness – Brinell290–322HB
Elastic stored energy (springs)964–1180kJ/m3
Fatigue strength at 10^7 cycles600–650MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
562–694MPa

PH 13-8Mo Impact & fracture properties

Fracture toughness172–210MPa.m0.5
Toughness (G)149–219kJ/m2

PH 13-8Mo H1150 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity14–15.2W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient10.4–11µstrain/°C
Thermal shock resistance287–324°C
Thermal distortion resistance1.3–1.43MW/m
Latent heat of fusion260–285kJ/kg

PH 13-8Mo Electrical properties

Electrical resistivity97–107µohm.cm
Electrical conductivity1.61–1.78%IACS
Galvanic potential-0.26–-0.18V

PH 13-8Mo Magnetic properties

Magnetic typeMagnetic

PH 13-8Mo Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5020–5150m/s
Mechanical loss coefficient (tan delta)2.7e-4–3.2e-4 

PH 13-8Mo Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed9.14 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.665 – 0.808

PH 13-8Mo Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

PH 13-8Mo H1150 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)18.8 – 21.6
Pitting and crevice corrosionMedium (20-30)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasRestricted

PH 13-8Mo Standards with similar compositions

USA: S13800 to ASTM A564/A564M, S13800 to ASTM A693, S13800 to ASTM A705/A705M-95, S13800 to ASTM A959, UNS S13800, UNS S13889
Tradenames: ARMCO PH 13-8 MO, CARPENTER PH 13-8 MO STAINLESS, CARPENTER TOURALLOY 230 PLUS, LESCALLOY 13-8 MO VIM-VAR, MARVAL 13 X, NIROSTA 4534, PRP-13-8 MO, UDIMET ALLOY 13-8MO, UNILOY 13-8