FV520 (BS S144) Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

FV520 (BS S144) Overview

FV520 BS S144 is a martensitic precipitation hardening stainless steel (EN 1.4594) in the wrought form. Condition: Solution treated at 1000°C, primary hardened at 800°C, precipitation hardened at 450°C. This FV520 BS S144 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for FV520 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined FV520 parts in-house and inspects them before shipment.

FV520 Designation

FV520 (BS S144), wrought
ConditionSolution treated at 1000°C, primary hardened at 800°C, precipitation hardened at 450°C
EN nameX5CrNiMoCuNb14-5 to BS EN 10088-1, BS EN 10088-3, BS S 143, BS S 144, BS S 145
EN number1.4594
TradenamesFirth Vickers FV520, FV520B

FV520 Typical uses

Blading, bolts, fasteners, valves, pumps, water impellers, and assemblies, in the aviation and aerospace industries, nuclear, turbine and general mechanical engineering.

FV520 (BS S144) Composition detail

C (carbon)0–0.07%
Cr (chromium)13.2–14.7%
Cu (copper)1.2–2%
Fe (iron)73.3–79.3%
Mn (manganese)0–1%
Mo (molybdenum)1.2–2%
Nb (niobium)0.1–0.4%
Ni (nickel)5–5.8%
P (phosphorus)0–0.035%
S (sulfur)0–0.025%
Si (silicon)0–0.7%

FV520 Physical properties

Density7.82–7.83g/cm3

FV520 (BS S144) Mechanical properties

Young’s modulus206–216GPa
Specific stiffness26.3–27.6MN.m/kg
Yield strength (elastic limit)1030–1200MPa
Tensile strength1130–1330MPa
Specific strength132–153kN.m/kg
Elongation12–18% strain
Compressive modulus206–216GPa
Compressive strength1030–1200MPa
Flexural modulus206–216GPa
Flexural strength (modulus of rupture)924–1090MPa
Shear modulus78–82GPa
Shear strength756–882MPa
Bulk modulus172–180GPa
Poisson’s ratio0.295–0.305 
Shape factor21.9
Hardness – Vickers370–420HV
Hardness – Rockwell C38–43HRC
Hardness – Brinell352–401HB
Elastic stored energy (springs)2520–3400kJ/m3
Fatigue strength at 10^7 cycles373–439MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
339–483MPa

FV520 Impact & fracture properties

Fracture toughness106–129MPa.m0.5
Toughness (G)53.7–78.3kJ/m2

FV520 (BS S144) Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity16.5–17.9W/m.°C
Specific heat capacity471–490J/kg.°C
Thermal expansion coefficient11–11.5µstrain/°C
Thermal shock resistance432–509°C
Thermal distortion resistance1.46–1.6MW/m
Latent heat of fusion266–327kJ/kg

FV520 Electrical properties

Electrical resistivity80–85µohm.cm
Electrical conductivity2.03–2.16%IACS

FV520 Magnetic properties

Magnetic typeMagnetic

FV520 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5130–5250m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

FV520 Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed10.4 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGFair
Weldability – plasmaGood
Weldability – SAWFair
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.912 – 1.21

FV520 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Limited use
FlammabilityNon-flammable

FV520 (BS S144) Corrosion resistance

Pitting resistance equivalent number (PREN)17.9 – 20.8
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Slightly susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasGood