Custom 465 H950 Stainless Steel Material Data Sheet

Custom 465 H950 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

Custom 465 H950 Stainless Steel Overview

Custom 465 H950 stainless steel is a martensitic precipitation hardening stainless steel (UNS S46500) in the wrought form. Condition: H950 (Solution annealed; precipitation (age) hardened at 510°C; air cooled). This Custom 465 H950 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 465 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 465 parts in-house and inspects them before shipment.

Custom 465 Designation

Custom 465, wrought
ConditionH950 (Solution annealed; precipitation (age) hardened at 510°C; air cooled)
UNS numberS46500
US nameCustom 465

Custom 465 H950 Stainless Steel Composition detail

C (carbon)0–0.02%
Cr (chromium)11–12.5%
Fe (iron)72.7–76%
Mn (manganese)0–0.25%
Mo (molybdenum)0.75–1.25%
Ni (nickel)10.8–11.2%
P (phosphorus)0–0.015%
S (sulfur)0–0.01%
Si (silicon)0–0.25%
Ti (titanium)1.5–1.8%

Custom 465 Physical properties

Density7.75–7.91g/cm3

Custom 465 H950 Stainless Steel Mechanical properties

Young’s modulus194–204GPa
Specific stiffness24.7–26MN.m/kg
Yield strength (elastic limit)1540–1670MPa
Tensile strength1660–1800MPa
Specific strength196–213kN.m/kg
Elongation5–14% strain
Compressive strength1580–1750MPa
Flexural modulus194–204GPa
Flexural strength (modulus of rupture)1540–1670MPa
Shear modulus76–79.5GPa
Bulk modulus143–158GPa
Poisson’s ratio0.274–0.286 
Shape factor14
Hardness – Vickers459–517HV
Hardness – Rockwell B115–119HRB
Hardness – Rockwell C47–53HRC
Hardness – Brinell458–507HB
Elastic stored energy (springs)5950–7040kJ/m3
Fatigue strength at 10^7 cycles688–760MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
650–804MPa

Custom 465 Impact & fracture properties

Fracture toughness67.5–82.5MPa.m0.5
Toughness (G)23.1–34kJ/m2

Custom 465 H950 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity14.7–16W/m.°C
Specific heat capacity490–510J/kg.°C
Thermal expansion coefficient10.2–10.8µstrain/°C
Thermal shock resistance729–812°C
Thermal distortion resistance1.39–1.53MW/m
Latent heat of fusion238–293kJ/kg

Custom 465 Electrical properties

Electrical resistivity80.7–83.9µohm.cm
Electrical conductivity2.05–2.14%IACS
Galvanic potential-0.27–-0.19V

Custom 465 Magnetic properties

Magnetic typeMagnetic

Custom 465 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4970–5100m/s
Mechanical loss coefficient (tan delta)3e-4–6.6e-4 

Custom 465 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed6.71 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.597 – 0.723

Custom 465 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

Custom 465 H950 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)13.5 – 16.6
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsRestricted
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasGood

Custom 465 Notes

Custom 465 H950 Warning
Certain processing procedures may cause these extrusions to become susceptible to stress-corrosion cracking
Custom 465 H950 Other notes
Custom 465® stainless is a double-vacuum melted, martensitic, age-hardenable alloy. This alloy was designed to have excellent notch tensile strength and fracture toughness over a wide range of section sizes. In the H950 condition, the alloy achieves a minimum ultimate tensile strength of 240 ksi while retaining good toughness and resistance to stress-corrosion cracking. Custom 465 stainless provides a superior combination of strength, toughness and stress corrosion cracking resistance compared with other high-strength PH stainless alloys such as Custom 455® stainless or PH13-8Mo® stainless.

Custom 465 Standards with similar compositions

USA: S46500 to ASTM A564/A564M, S46500 to ASTM A693, S46500 to ASTM A959, UNS S46500