15-5PH H900 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
15-5PH H900 Stainless Steel Overview
15-5PH H900 stainless steel is a martensitic precipitation hardening stainless steel (UNS S15500) in the wrought form. Condition: H900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled). This 15-5PH H900 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 15-5PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 15-5PH parts in-house and inspects them before shipment.
15-5PH Designation
15-5PH, wrought
Condition
H900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled)
UNS number
S15500
US name
15-5PH
15-5PH Typical uses
Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
15-5PH H900 Stainless Steel Composition detail
C (carbon)
0
–
0.07
%
Cr (chromium)
14
–
15.5
%
Cu (copper)
2.5
–
4.5
%
Fe (iron)
71.9
–
79.8
%
Mn (manganese)
0
–
1
%
Nb (niobium)
0.15
–
0.4
%
Ni (nickel)
3.5
–
5.5
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0
–
0.03
%
Si (silicon)
0
–
1
%
Ta (tantalum)
0
–
0.05
%
15-5PH Physical properties
Density
7.79
–
7.87
g/cm3
15-5PH H900 Stainless Steel Mechanical properties
Young’s modulus
197
–
207
GPa
Specific stiffness
25.1
–
26.5
MN.m/kg
Yield strength (elastic limit)
1170
–
1300
MPa
Tensile strength
1310
–
1450
MPa
Specific strength
150
–
165
kN.m/kg
Elongation
13
–
15.1
% strain
Compressive strength
986
–
1090
MPa
Flexural modulus
197
–
207
GPa
Flexural strength (modulus of rupture)
1170
–
1300
MPa
Shear modulus
77
–
80.9
GPa
Bulk modulus
142
–
150
GPa
Poisson’s ratio
0.27
–
0.281
Shape factor
19
Hardness – Vickers
250
–
460
HV
Hardness – Rockwell B
113
–
116
HRB
Hardness – Rockwell C
42
–
47
HRC
Hardness – Brinell
398
–
442
HB
Elastic stored energy (springs)
3400
–
4160
kJ/m3
Fatigue strength at 10^7 cycles
364
–
542
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357
–
552
MPa
15-5PH Impact & fracture properties
Fracture toughness
79.7
–
97.4
MPa.m0.5
Toughness (G)
31.7
–
46.5
kJ/m2
15-5PH H900 Stainless Steel Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
282
–
316
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
17.8
–
19.3
W/m.°C
Specific heat capacity
440
–
458
J/kg.°C
Thermal expansion coefficient
10.6
–
11.2
µstrain/°C
Thermal shock resistance
527
–
595
°C
Thermal distortion resistance
1.62
–
1.78
MW/m
Latent heat of fusion
260
–
285
kJ/kg
15-5PH Electrical properties
Electrical resistivity
72
–
82
µohm.cm
Electrical conductivity
2.1
–
2.39
%IACS
Galvanic potential
-0.22
–
-0.14
V
15-5PH Magnetic properties
Magnetic type
Magnetic
15-5PH Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5010
–
5140
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
15-5PH Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Unsuitable
Machining speed
12.2 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIG
Good
Weldability – plasma
Good
Weldability – SAW
Not recommended
Weldability – TIG
Good
Brazeability
Good
Carbon equivalency
0.608 – 0.895
15-5PH Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aging martensitic steels at a low temperatures, around 480 °C, improves resistance. Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
15-5PH H900 Stainless Steel Corrosion resistance
Pitting resistance equivalent number (PREN)
14 – 15.5
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Slightly susceptible
Intergranular (weld line) corrosion
Good
Inorganic acids
Restricted
Organic acids
Moderate
Alkalis
Moderate
Humidity / water
Excellent
Sea water
Restricted
Sour oil and gas
Restricted
15-5PH Standards with similar compositions
China: 0Cr16Ni4Cu4Nb to GB 8732
France: Z6CNU15.05 to AFNOR NF A35-581
Germany: GX4CrNiCuNb16-4 to DIN
USA: 17-4PH to SAE J467, 5658 to AMS 5658, 5659 to AMS 5659, 5826 to AMS 5826, 5862 to AMS 5862, S15500 to ASTM A564/A564M, S15500 to ASTM A693, S15500 to ASTM A705/A705M-95, S15500 to ASTM A959, UNS J92110, UNS S15500