PEK 30% Glass Fiber Material Data Sheet

PEK 30% Glass Fiber (Polyetherketone) Material Data Sheet

PEK 30% Glass Fiber Overview

PEK 30% glass fiber is a grade of polyetherketone (PEK), designated Polyetherketone (30% Glass Fiber). This PEK 30% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEK parts in-house and inspects them before shipment.

PEK Designation

Polyetherketone (30% Glass Fiber)
TradenamesArylmax, Avaspire, G-Paek, Victrex

PEK Typical uses

Bearing cages, gear support bearings, thrust washers, clutch seals, transmission parts, housing for tire pressure sensors, valve spring discs, rollers, guides, gears, reciprocating components.

PEK 30% Glass Fiber Composition detail

Polymer70  %
Glass (fiber)30  %

PEK Physical properties

Density1.47–1.53g/cm3

PEK 30% Glass Fiber Mechanical properties

Young’s modulus9.72–12.1GPa
Specific stiffness6.47–8.08MN.m/kg
Yield strength (elastic limit)130–152MPa
Tensile strength163–190MPa
Specific strength86.7–102kN.m/kg
Elongation2.2–3.4% strain
Compressive modulus9.72–12.1GPa
Compressive strength197–217MPa
Flexural modulus10.7–11.3GPa
Flexural strength (modulus of rupture)235–250MPa
Shear modulus3.6–4.48GPa
Bulk modulus11.8–12.4GPa
Poisson’s ratio0.344–0.358 
Shape factor6.9
Hardness – Vickers39–46HV
Hardness – Rockwell M97–107 
Hardness – Rockwell R120–132 
Elastic stored energy (springs)763–1090kJ/m3
Fatigue strength at 10^7 cycles76–84MPa

PEK Impact & fracture properties

Fracture toughness4.94–7.55MPa.m0.5
Toughness (G)2.31–5.11kJ/m2
Impact strength, notched 23 °C9.09–11kJ/m2
Impact strength, notched -30 °C8.18–9.9kJ/m2
Impact strength, unnotched 23 °C63.6–77kJ/m2
Impact strength, unnotched -30 °C68.2–82.5kJ/m2

PEK 30% Glass Fiber Thermal properties

Melting point329–381°C
Glass temperature182–200°C
Heat deflection temperature 0.45MPa340–350°C
Heat deflection temperature 1.8MPa326–350°C
Vicat softening point340–350°C
Maximum service temperature235–255°C
Minimum service temperature-47–-27°C
Thermal conductivity0.494–0.513W/m.°C
Specific heat capacity1310–1370J/kg.°C
Thermal expansion coefficient33.3–36µstrain/°C
Thermal shock resistance327–430°C
Thermal distortion resistance0.0139–0.0152MW/m

PEK Electrical properties

Electrical resistivity3300000000000000000000–30000000000000000000000µohm.cm
Electrical conductivity5.75e-21–5.22e-20%IACS
Dielectric constant (relative permittivity)3.14–3.46 
Dissipation factor (dielectric loss tangent)0.00398–0.00477 
Dielectric strength (dielectric breakdown)14–15.1MV/m
Comparative tracking index175–225V

PEK Magnetic properties

Magnetic typeNon-magnetic

PEK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2540–2850m/s
Mechanical loss coefficient (tan delta)0.00698–0.00814 

PEK Absorption & permeability

Water absorption @ 24 hrs0.06–0.08%

PEK Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 0.9 %
Melt temperature334 – 429 °C
Molding pressure range68.8 – 138 MPa

PEK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySelf-extinguishing

PEK Notes

PEK 30% Glass Fiber Other notes
Endurance limit tested at 15 Hz