Modified PEK 40% Glass Fiber Material Data Sheet

Modified PEK 40% Glass Fiber (Polyetherketone) Material Data Sheet

Modified PEK 40% Glass Fiber Overview

Modified PEK 40% glass fiber is a grade of polyetherketone (PEK), designated Polyetherketone (Modified, 40% Glass Fiber). This modified PEK 40% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEK parts in-house and inspects them before shipment.

Modified PEK Designation

Polyetherketone (Modified, 40% Glass Fiber)
TradenamesAvaspire

Modified PEK Typical uses

Bearing cages, gear support bearings, thrust washers, clutch seals, transmission parts, housing for tire pressure sensors, valve spring discs, rollers, guides, gears, reciprocating components.

Modified PEK 40% Glass Fiber Composition detail

Polymer60  %
Glass (fiber)40  %

Modified PEK Physical properties

Density1.58–1.62g/cm3

Modified PEK 40% Glass Fiber Mechanical properties

Young’s modulus15.1–15.9GPa
Specific stiffness9.41–9.97MN.m/kg
Yield strength (elastic limit)118–130MPa
Tensile strength148–163MPa
Specific strength73.9–81.6kN.m/kg
Elongation1.4–1.61% strain
Compressive modulus15.1–15.9GPa
Compressive strength217–239MPa
Flexural modulus14.1–14.8GPa
Flexural strength (modulus of rupture)223–246MPa
Shear modulus5.65–5.94GPa
Bulk modulus15.5–16.3GPa
Poisson’s ratio0.331–0.344 
Shape factor9.5
Hardness – Vickers36–39HV
Hardness – Rockwell M98–108 
Hardness – Rockwell R120–132 
Elastic stored energy (springs)452–549kJ/m3
Fatigue strength at 10^7 cycles54.6–70.9MPa

Modified PEK Impact & fracture properties

Fracture toughness4.55–5.46MPa.m0.5
Toughness (G)1.34–1.91kJ/m2
Impact strength, notched 23 °C6–6.6kJ/m2

Modified PEK 40% Glass Fiber Thermal properties

Melting point312–336°C
Glass temperature182–200°C
Heat deflection temperature 0.45MPa310–370°C
Heat deflection temperature 1.8MPa280–337°C
Vicat softening point310–370°C
Maximum service temperature231–252°C
Minimum service temperature-47–-27°C
Thermal conductivity0.354–0.383W/m.°C
Specific heat capacity1250–1300J/kg.°C
Thermal expansion coefficient32.6–34µstrain/°C
Thermal shock resistance227–255°C
Thermal distortion resistance0.0106–0.0116MW/m

Modified PEK Electrical properties

Electrical resistivity3300000000000000000000–30000000000000000000000µohm.cm
Electrical conductivity5.75e-21–5.22e-20%IACS
Dielectric constant (relative permittivity)3.14–3.46 
Dissipation factor (dielectric loss tangent)0.00398–0.00477 
Dielectric strength (dielectric breakdown)14.6–15.8MV/m
Comparative tracking index175–225V

Modified PEK Magnetic properties

Magnetic typeNon-magnetic

Modified PEK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3070–3160m/s
Mechanical loss coefficient (tan delta)0.00577–0.00598 

Modified PEK Absorption & permeability

Water absorption @ 24 hrs0.0364–0.044%

Modified PEK Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 0.9 %
Melt temperature323 – 407 °C
Molding pressure range68.8 – 138 MPa

Modified PEK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySelf-extinguishing