AISI 1025 normalized is AISI 1025 low carbon steel (UNS G10250) in the normalized condition. This AISI 1025 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for AISI 1025 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1025 steel parts in-house and inspects them before shipment.
AISI 1025 Normalized Designation
AISI 1025
Condition
Normalized
UNS number
G10250
US name
ASME 1025, ASTM M1025, ASTM 1025, ASME G10250, SAE 850, AMS 5045, ~SAE 853 Class 1 Type 5, ~SAE 853 Class 1 Type 4, ~SAE 853 Class 1 Type 3, ~SAE 853 Class 1 Type 2, ~SAE 853 Class 1 Type 1, ~SAE 040S, ~SAE 040C, ~SAE 040B, ~SAE 040A, ~ASTM FPA
General engineering, structural and mechanical engineering.
AISI 1025 Normalized Composition detail
C (carbon)
0.22
–
0.28
%
Fe (iron)
99
–
99.5
%
Mn (manganese)
0.3
–
0.6
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0
–
0.05
%
AISI 1025 Normalized Physical properties
Density
7.82
–
7.9
g/cm3
AISI 1025 Normalized Mechanical properties
Young’s modulus
200
–
210
GPa
Specific stiffness
25.4
–
26.8
MN.m/kg
Yield strength (elastic limit)
248
–
274
MPa
Tensile strength
379
–
419
MPa
Specific strength
31.5
–
34.9
kN.m/kg
Elongation
25
–
40
% strain
Compressive strength
248
–
274
MPa
Flexural modulus
200
–
210
GPa
Flexural strength (modulus of rupture)
248
–
274
MPa
Shear modulus
76
–
79.9
GPa
Bulk modulus
185
–
195
GPa
Poisson’s ratio
0.32
–
0.333
Shape factor
62
Hardness – Vickers
108
–
173
HV
Elastic stored energy (springs)
150
–
183
kJ/m3
Fatigue strength at 10^7 cycles
203
–
293
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
197
–
303
MPa
AISI 1025 Normalized Impact & fracture properties
Fracture toughness
41
–
82
MPa.m0.5
Toughness (G)
8.96
–
30
kJ/m2
AISI 1025 Normalized Thermal properties
Melting point
1480
–
1530
°C
Maximum service temperature
432
–
482
°C
Minimum service temperature
-68
–
-38
°C
Thermal conductivity
51.9
–
56.2
W/m.°C
Specific heat capacity
486
–
506
J/kg.°C
Thermal expansion coefficient
11.3
–
11.9
µstrain/°C
Thermal shock resistance
103
–
116
°C
Thermal distortion resistance
4.43
–
4.87
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 1025 Normalized Electrical properties
Electrical resistivity
15
–
20
µohm.cm
Electrical conductivity
8.62
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 1025 Normalized Magnetic properties
Magnetic type
Magnetic
AISI 1025 Normalized Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5040
–
5170
m/s
Mechanical loss coefficient (tan delta)
0.0011
–
0.0014
AISI 1025 Normalized Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
39.6 m/min
Weldability Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency
0.27 – 0.38
AISI 1025 Normalized Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 1025 Normalized Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible
AISI 1025 Normalized Notes
AISI 1025 Normalized Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges.
AISI 1025 Normalized Standards with similar compositions
China: ML25 to GB/T 6478
India: 25C4 to IS 11169/1, 25C4 to IS 1570/2/1, C25 to IS 1570/2/1, CEW-2 to IS 3074, ERW-2 to IS 3074, Grade 10 to IS 7887, Grade 10 to IS 8952, Grade 9 to IS 7887, Grade 9 to IS 8952
Japan: SGD 4 to JIS G3108, SWRM 22 to JIS G3505
Mexico: 1023 to NMX-B-301, 1025 to NMX-B-201, 1025 to NMX-B-203-SCFI, 1025 to NMX-B-301
Pan America: 1023 to COPANT 333, 1025 to COPANT 330, 1025 to COPANT 331, 1025 to COPANT 333
South Korea: SGD 4 to KS D 3526, SWRM 22 to KS D 3554
UK: HS22 to BS 1449 Section 1.14
USA: 1023, 1023 to ASTM A29/A29M, 1023 to SAE J403, 1025, 1025 to ASTM A29/A29M, 1025 to ASTM A512-96, 1025 to ASTM A513, 1025 to ASTM A519, 1025 to ASTM A568/A568M, 1025 to MIL-S-11310E, 1025 to MIL-S-7952A, 1025 to MIL-T-3520, 1025 to SAE J403, A to MIL-T-20157, B to MIL-T-20157, C to MIL-T-20157, D to MIL-T-20157, G10230 to ASTM A510/A510M, G10230 to ASTM A576-90b, G10230 to ASTM A830/A830M, G10250 to ASTM A510/A510M, G10250 to ASTM A576-90b, G10250 to ASTM A830/A830M, G10250 to FED QQ-S-700D, M1023, M1023 to ASTM A29/A29M, M1023 to ASTM A575-96, M1023 to SAE J403, M1025, M1025 to ASTM A29/A29M, M1025 to ASTM A575-96, M1025 to SAE J403, UNS G10230, UNS G10230 to UNS, UNS G10250, UNS G10250 to UNS, UNS K02706