Home » High Conductivity Copper » C18200 H.C. Copper, Solution Treated & Work Hardened Material Data Sheet
C18200 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Work Hardened)
C18200 Solution Treated Cold Worked Copper Overview
C18200 solution treated cold worked copper is a wrought high conductivity copper (UNS C18200, EN CW105C), known as h.c. copper. Condition: Solution heat-treated & work hardened. This C18200 solution treated cold worked copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C18200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C18200 copper parts in-house and inspects them before shipment.
C18200 Designation
Copper Alloy: hc-CuCr1(wh); A2/1 (UNS C18200) Condition Solution heat-treated & work hardened UNS number C18200 EN name CW105C ISO name CuCr1 JIS (Japanese) name C1820
C18200 Typical uses
Cable connectors, switchgear & circuit breakers, commutator bars & end-rings for electrical motors, electronic devices, contact wheels.
C18200 Solution Treated Cold Worked Copper Composition detail
Cr (chromium) 0.6 – 1.2 % Cu (copper) 98.6 – 99.4 % Fe (iron) 0 – 0.1 % Pb (lead) 0 – 0.05 % Si (silicon) 0 – 0.1 %
C18200 Physical properties
C18200 Solution Treated Cold Worked Copper Mechanical properties
Young’s modulus 110 – 115 GPa Specific stiffness 12.3 – 12.9 MN.m/kg Yield strength (elastic limit) 180 – 290 MPa Tensile strength 350 – 510 MPa Specific strength 20.1 – 32.4 kN.m/kg Elongation 4 – 7 % strain Compressive strength 180 – 290 MPa Flexural modulus 110 – 115 GPa Flexural strength (modulus of rupture) 180 – 290 MPa Shear modulus 41 – 42 GPa Bulk modulus 119 – 124 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 27 Hardness – Vickers 115 – 130 HV Elastic stored energy (springs) 151 – 357 kJ/m3 Fatigue strength at 10^7 cycles 160 – 180 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 120 – 241 MPa
C18200 Impact & fracture properties
Fracture toughness 43.2 – 57.6 MPa.m0.5 Toughness (G) 16.9 – 29 kJ/m2
C18200 Solution Treated Cold Worked Copper Thermal properties
Melting point 1070 – 1080 °C Maximum service temperature 300 – 350 °C Minimum service temperature -273 °C Thermal conductivity 160 – 170 W/m.°C Specific heat capacity 372 – 380 J/kg.°C Thermal expansion coefficient 16.9 – 17.1 µstrain/°C Thermal shock resistance 94.1 – 152 °C Thermal distortion resistance 9.41 – 10 MW/m Latent heat of fusion 200 – 208 kJ/kg
C18200 Electrical properties
Electrical resistivity 4.9 – 5.13 µohm.cm Electrical conductivity 33.6 – 35.2 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.19 – -0.11 V
C18200 Magnetic properties
Magnetic type Non-magnetic
C18200 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3510 – 3590 m/s Mechanical loss coefficient (tan delta) 4.8e-5 – 1.23e-4
C18200 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Acceptable Metal press forming Excellent Metal deep drawing Limited use Machining speed 33.5 m/min Weldability Notes: Preheating and post weld heat treatment are not required Good
C18200 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C18200 Solution Treated Cold Worked Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C18200 Notes
C18200 Solution Treated Cold Worked Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C18200 Standards with similar compositions
Europe: CW105C to CEN EN 12163, CW105C to CEN EN 12165, CW105C to CEN EN 12167, CW105C to CEN EN 12420Germany: 2.1291 to DIN, CuCrZr to DINInternational: CuCr1 to ISO 1637, CuCr1 to ISO 1640, CuCr1 to ISO R1336Japan: CuCr1 to JIS Z3234USA: 99Cu-1Cr to ASTM F9, C18200, UNS C18200Tradenames: AMCROM, AMPCOLOY 98, AMPCO-TRODE 182, ANACONDA 182, BOLTOMET 814, BOLTOMET 818, BRUSH CHROMIUM COPPER, CERRO CCS, CHROMIUM COPPER-182, CHROMIUM-COPPER 999, CUPROCHROME, ERM CCS, ERM CCS (M3), HIDUREL 6, MITSUBISHI MKC, MUELLER 1820