High Conductivity Copper Material Data Sheet (Cast)
Cast High Conductivity Copper Overview
Cast high conductivity copper is a cast high conductivity copper, known as h.c. copper. Condition: Cast. This cast high conductivity copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for high conductivity copper castings from Turkey (Türkiye)? Modulus Metal supplies high conductivity copper castings with in-house CNC machining and inspects them before shipment.
H.C. Copper Designation
Copper Alloy: hc-Cu
H.C. Copper Typical uses
Castings, electrical components, fittings for liquid gases.
Cast High Conductivity Copper Composition detail
C (carbon)
0
–
0.1
%
Cu (copper)
99.9
–
100
%
H.C. Copper Physical properties
Density
8.94
–
8.95
g/cm3
Cast High Conductivity Copper Mechanical properties
Young’s modulus
122
–
128
GPa
Specific stiffness
13.6
–
14.3
MN.m/kg
Yield strength (elastic limit)
28
–
40
MPa
Tensile strength
145
–
160
MPa
Specific strength
3.13
–
4.47
kN.m/kg
Elongation
23
–
25
% strain
Compressive strength
28
–
40
MPa
Flexural modulus
122
–
128
GPa
Flexural strength (modulus of rupture)
28
–
40
MPa
Shear modulus
45.1
–
47.4
GPa
Bulk modulus
132
–
138
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
43
–
46
HV
Elastic stored energy (springs)
3.22
–
6.23
kJ/m3
Fatigue strength at 10^7 cycles
91
–
97
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
84.9
–
104
MPa
H.C. Copper Impact & fracture properties
Fracture toughness
100
–
107
MPa.m0.5
Toughness (G)
79.8
–
91.4
kJ/m2
Cast High Conductivity Copper Thermal properties
Melting point
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
390
–
398
W/m.°C
Specific heat capacity
383
–
387
J/kg.°C
Thermal expansion coefficient
16.8
–
16.9
µstrain/°C
Thermal shock resistance
13.3
–
19
°C
Thermal distortion resistance
23.1
–
23.6
MW/m
Latent heat of fusion
200
–
208
kJ/kg
H.C. Copper Electrical properties
Electrical resistivity
1.91
–
1.95
µohm.cm
Electrical conductivity
88.4
–
90.3
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
H.C. Copper Magnetic properties
Magnetic type
Non-magnetic
H.C. Copper Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3690
–
3780
m/s
Mechanical loss coefficient (tan delta)
0.0025
–
0.0051
H.C. Copper Processing properties
Metal casting
Limited use
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
29.3 m/min
Weldability Notes: Preheating and post weld heat treatment are not required
Good
H.C. Copper Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
Cast High Conductivity Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
H.C. Copper Notes
Cast High Conductivity Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
H.C. Copper Standards with similar compositions
Japan: CAC101 to JIS H5120, CAC102 to JIS H5120, CAC103 to JIS H5120
USA: C81200, UNS C80300, UNS C80500, UNS C80700, UNS C80900, UNS C81200
Tradenames: LEADED GUN METAL, PHOSPHOR COPPER GRADE B