C14700 H.C. Copper, Hard Material Data Sheet

C14700 H.C. Copper Material Data Sheet (Wrought, Hard)

C14700 Hard Copper Overview

C14700 hard copper is a wrought high conductivity copper (UNS C14700, EN CW114C), known as h.c. copper. Condition: Hard. This C14700 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14700 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14700 copper parts in-house and inspects them before shipment.

C14700 Designation

Wrought Copper Alloy: hc-CuS(h); C111 (UNS C14700)
ConditionHard
UNS numberC14700
EN nameCW114C
ISO nameCuS(P0,03)

C14700 Hard Copper Composition detail

Cu (copper)99.5–99.8%
P (phosphorus)0.002–0.005%
S (sulfur)0.2–0.5%

C14700 Physical properties

Density8.94–8.95g/cm3

C14700 Hard Copper Mechanical properties

Young’s modulus128–135GPa
Specific stiffness14.3–15.1MN.m/kg
Yield strength (elastic limit)230–320MPa
Tensile strength270–350MPa
Specific strength25.7–35.8kN.m/kg
Elongation5–15% strain
Compressive strength230–320MPa
Flexural modulus128–135GPa
Flexural strength (modulus of rupture)230–320MPa
Shear modulus45–50GPa
Bulk modulus138–146GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers85–110HV
Elastic stored energy (springs)206–381kJ/m3
Fatigue strength at 10^7 cycles90–105MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
75–126MPa

C14700 Impact & fracture properties

Fracture toughness40.4–50MPa.m0.5
Toughness (G)12.5–18.8kJ/m2

C14700 Hard Copper Thermal properties

Melting point1070–1080°C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity365–370W/m.°C
Specific heat capacity377–383J/kg.°C
Thermal expansion coefficient17–18µstrain/°C
Thermal shock resistance99.7–140°C
Thermal distortion resistance20.4–21.6MW/m
Latent heat of fusion200–208kJ/kg

C14700 Electrical properties

Electrical resistivity1.82–1.86µohm.cm
Electrical conductivity92.7–94.7%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C14700 Magnetic properties

Magnetic typeNon-magnetic

C14700 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3780–3890m/s
Mechanical loss coefficient (tan delta)3.9e-5–7.6e-5 

C14700 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Poor

C14700 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C14700 Hard Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C14700 Notes

C14700 Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C14700 Standards with similar compositions

Australia: 147 to AS 1567, C14700 to AS 2738
Europe: CW114C to CEN EN 12164, CW114C to CEN EN 12168
Germany: 2.1498 to DIN, CuSP to DIN
International: CuS(P0.01) to ISO 1637, CuS(P0.01) to ISO R1336, CuS(P0.03) to ISO 1637, CuS(P0.03) to ISO R1336
UK: C111 to BS 2874
USA: C14700, C14700 to ASTM B124M, C14700 to ASTM B283, C14700 to ASTM B301/B301M, C14700 to SAE J463, UNS C14700, UNS C14720
Tradenames: AMSULF, BOLTOMET 917, BRIDGEPORT NO. 120, ERM CUS, MCKECHNIE SC, MUELLER 1470, MUELLER 1476, OFHC SULFUR COPPER, OSNA CU58S, SCOVILL NO. 1032, SULPH-COPPER