C18200 H.C. Copper, Solution Treated & Aged Material Data Sheet

C18200 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Aged)

C18200 Solution Treated Aged Copper Overview

C18200 solution treated aged copper is a wrought high conductivity copper (UNS C18200, EN CW105C), known as h.c. copper. Condition: Solution heat-treated & precipitation hardened. This C18200 solution treated aged copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C18200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C18200 copper parts in-house and inspects them before shipment.

C18200 Designation

Copper Alloy: hc-CuCr1(wp) (UNS C18200)
ConditionSolution heat-treated & precipitation hardened
UNS numberC18200
EN nameCW105C
ISO nameCuCr1
JIS (Japanese) nameC1820

C18200 Typical uses

Cable connectors, switchgear & circuit breakers, commutator bars & end-rings for electrical motors, electronic devices, contact wheels.

C18200 Solution Treated Aged Copper Composition detail

Cr (chromium)0.6–1.2%
Cu (copper)98.6–99.4%
Fe (iron)0–0.1%
Pb (lead)0–0.05%
Si (silicon)0–0.1%

C18200 Physical properties

Density8.94–8.95g/cm3

C18200 Solution Treated Aged Copper Mechanical properties

Young’s modulus140–150GPa
Specific stiffness15.7–16.8MN.m/kg
Yield strength (elastic limit)290–310MPa
Tensile strength405–420MPa
Specific strength32.4–34.7kN.m/kg
Elongation14–16% strain
Compressive strength290–310MPa
Flexural modulus140–150GPa
Flexural strength (modulus of rupture)290–310MPa
Shear modulus52–55GPa
Bulk modulus151–162GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers130–138HV
Elastic stored energy (springs)288–334kJ/m3
Fatigue strength at 10^7 cycles170–200MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
169–202MPa

C18200 Impact & fracture properties

Fracture toughness41.3–43.2MPa.m0.5
Toughness (G)11.6–13kJ/m2

C18200 Solution Treated Aged Copper Thermal properties

Melting point1070–1080°C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity300–340W/m.°C
Specific heat capacity372–380J/kg.°C
Thermal expansion coefficient16.9–17.1µstrain/°C
Thermal shock resistance116–128°C
Thermal distortion resistance17.6–20MW/m
Latent heat of fusion200–208kJ/kg

C18200 Electrical properties

Electrical resistivity2–2.29µohm.cm
Electrical conductivity75.3–86.2%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.19–-0.11V

C18200 Magnetic properties

Magnetic typeNon-magnetic

C18200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3960–4100m/s
Mechanical loss coefficient (tan delta)4.2e-5–4.8e-5 

C18200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C18200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C18200 Solution Treated Aged Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C18200 Notes

C18200 Solution Treated Aged Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C18200 Standards with similar compositions

Europe: CW105C to CEN EN 12163, CW105C to CEN EN 12165, CW105C to CEN EN 12167, CW105C to CEN EN 12420
Germany: 2.1291 to DIN, CuCrZr to DIN
International: CuCr1 to ISO 1637, CuCr1 to ISO 1640, CuCr1 to ISO R1336
Japan: CuCr1 to JIS Z3234
USA: 99Cu-1Cr to ASTM F9, C18200, UNS C18200
Tradenames: AMCROM, AMPCOLOY 98, AMPCO-TRODE 182, ANACONDA 182, BOLTOMET 814, BOLTOMET 818, BRUSH CHROMIUM COPPER, CERRO CCS, CHROMIUM COPPER-182, CHROMIUM-COPPER 999, CUPROCHROME, ERM CCS, ERM CCS (M3), HIDUREL 6, MITSUBISHI MKC, MUELLER 1820