Home » Gunmetal Alloys » CuSn7Zn2Ni5 Nickel Gunmetal, Cast Material Data Sheet
CuSn7Zn2Ni5 Nickel Gunmetal, Cast Material Data Sheet
CuSn7Zn2Ni5 Nickel Gunmetal Material Data Sheet (Cast)
CuSn7Zn2Ni5 Cast Gunmetal Overview
CuSn7Zn2Ni5 cast gunmetal is a cast gunmetal, known as nickel gunmetal. Condition: Cast. This CuSn7Zn2Ni5 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuSn7Zn2Ni5 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies CuSn7Zn2Ni5 gunmetal castings with in-house CNC machining and inspects them before shipment.
CuSn7Zn2Ni5 Designation
Copper Alloy: CuSn7Zn2Ni5
CuSn7Zn2Ni5 Typical uses
Pumps and valves, bearings, valve guides, marine uses, applications in high so2 atmospheres, slow-moving bearings, liners, bearing cages, switch parts, trolley hangers.
CuSn7Zn2Ni5 Cast Gunmetal Composition detail
Cu (copper)
86
%
Ni (nickel)
5.5
%
Sn (tin)
7
%
Zn (zinc)
2
%
CuSn7Zn2Ni5 Physical properties
Density
8.75
–
8.85
g/cm3
CuSn7Zn2Ni5 Cast Gunmetal Mechanical properties
Young’s modulus
79
–
82
GPa
Specific stiffness
8.97
–
9.33
MN.m/kg
Yield strength (elastic limit)
140
–
160
MPa
Tensile strength
280
–
340
MPa
Specific strength
15.9
–
18.2
kN.m/kg
Elongation
16
–
25
% strain
Compressive strength
140
–
160
MPa
Flexural modulus
79
–
82
GPa
Flexural strength (modulus of rupture)
140
–
160
MPa
Shear modulus
29.2
–
30.3
GPa
Bulk modulus
85.3
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
70
–
95
HV
Elastic stored energy (springs)
122
–
159
kJ/m3
Fatigue strength at 10^7 cycles
140
–
159
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
122
–
182
MPa
CuSn7Zn2Ni5 Impact & fracture properties
Fracture toughness
61.3
–
65.5
MPa.m0.5
Toughness (G)
46.6
–
53.4
kJ/m2
CuSn7Zn2Ni5 Cast Gunmetal Thermal properties
Melting point
917
–
1040
°C
Maximum service temperature
97
–
110
°C
Minimum service temperature
-63
–
-48
°C
Thermal conductivity
63
–
65
W/m.°C
Specific heat capacity
383
–
384
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
96
–
111
°C
Thermal distortion resistance
3.45
–
3.67
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuSn7Zn2Ni5 Electrical properties
Electrical resistivity
14.5
–
15.8
µohm.cm
Electrical conductivity
10.9
–
11.9
%IACS
Galvanic potential
-0.24
–
-0.16
V
CuSn7Zn2Ni5 Magnetic properties
Magnetic type
Non-magnetic
CuSn7Zn2Ni5 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2990
–
3050
m/s
Mechanical loss coefficient (tan delta)
1.56e-4
–
2.04e-4
CuSn7Zn2Ni5 Processing properties
Metal casting
Acceptable
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
27.7 m/min
Weldability
Unsuitable
CuSn7Zn2Ni5 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuSn7Zn2Ni5 Cast Gunmetal Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
CuSn7Zn2Ni5 Notes
CuSn7Zn2Ni5 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.