CuSn2ZnPb (C83810) Leaded Gunmetal, Cast Material Data Sheet

CuSn2ZnPb (C83810) Leaded Gunmetal Material Data Sheet (Cast)

C83810 Cast Gunmetal Overview

C83810 cast gunmetal is a cast gunmetal (UNS C83810), known as leaded gunmetal. Condition: Cast. This C83810 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C83810 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C83810 gunmetal castings with in-house CNC machining and inspects them before shipment.

C83810 Designation

CuSn2ZnPb
UNS numberC83810
ISO nameCuSn3Zn8Pb5

C83810 Typical uses

Pumps, valves, housings to resist corrosion, low-stressed bushings.

C83810 Cast Gunmetal Composition detail

Al (aluminum)0–0.01%
As (arsenic)0–0.5%
Bi (bismuth)0–0.1%
Cu (copper)77.4–86.5%
Fe (iron)0–0.5%
Ni (nickel)0–2%
Pb (lead)4–6%
Sb (antimony)0–0.5%
Si (silicon)0–0.005%
Sn (tin)2–3.5%
Zn (zinc)7.5–9.5%

C83810 Physical properties

Density8.75–8.85g/cm3

C83810 Cast Gunmetal Mechanical properties

Young’s modulus79–82GPa
Specific stiffness8.97–9.33MN.m/kg
Yield strength (elastic limit)80–130MPa
Tensile strength180–270MPa
Specific strength9.09–14.8kN.m/kg
Elongation2–8% strain
Compressive strength80–130MPa
Flexural modulus79–82GPa
Flexural strength (modulus of rupture)80–130MPa
Shear modulus29.2–30.3GPa
Bulk modulus85.3–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers65–80HV
Elastic stored energy (springs)41.7–100kJ/m3
Fatigue strength at 10^7 cycles105–137MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
81.4–177MPa

C83810 Impact & fracture properties

Fracture toughness67.9–82.6MPa.m0.5
Toughness (G)57.7–84.1kJ/m2

C83810 Cast Gunmetal Thermal properties

Melting point927–1070°C
Maximum service temperature180–190°C
Minimum service temperature-63–-48°C
Thermal conductivity74–76W/m.°C
Specific heat capacity383–384J/kg.°C
Thermal expansion coefficient17.5–18.5µstrain/°C
Thermal shock resistance55.2–89.9°C
Thermal distortion resistance4.04–4.3MW/m
Latent heat of fusion220–240kJ/kg

C83810 Electrical properties

Electrical resistivity10.7–14.5µohm.cm
Electrical conductivity11.9–16.1%IACS
Galvanic potential-0.26–-0.18V

C83810 Magnetic properties

Magnetic typeNon-magnetic

C83810 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2990–3050m/s
Mechanical loss coefficient (tan delta)2.37e-4–6.25e-4 

C83810 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed122 m/min
WeldabilityUnsuitable

C83810 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

C83810 Cast Gunmetal Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible

C83810 Notes

C83810 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C83810 Standards with similar compositions

Australia: 838C to AS 1565, C83810A to AS 2738
Europe: CB490K to CEN EN 1982, CC490K to CEN EN 1982
South Africa: Cu-Sn3Zn9Pb5 to SABS 200
USA: C83810, UNS C83810