CuSn7Zn2Ni5 Nickel Gunmetal, Cast, Aged Material Data Sheet

CuSn7Zn2Ni5 Nickel Gunmetal Material Data Sheet (Cast, Aged)

CuSn7Zn2Ni5 Cast Aged Gunmetal Overview

CuSn7Zn2Ni5 cast aged gunmetal is a cast gunmetal, known as nickel gunmetal. Condition: Aged. This CuSn7Zn2Ni5 cast aged gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuSn7Zn2Ni5 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies CuSn7Zn2Ni5 gunmetal castings with in-house CNC machining and inspects them before shipment.

CuSn7Zn2Ni5 Designation

Copper Alloy: CuSn7Zn2Ni5
ConditionAged

CuSn7Zn2Ni5 Typical uses

Pumps and valves, bearings, valve guides, marine uses, applications in high so2 atmospheres, slow-moving bearings, liners, bearing cages, switch parts, trolley hangers.

CuSn7Zn2Ni5 Cast Aged Gunmetal Composition detail

Cu (copper)86  %
Ni (nickel)5.5  %
Sn (tin)7  %
Zn (zinc)2  %

CuSn7Zn2Ni5 Physical properties

Density8.75–8.85g/cm3

CuSn7Zn2Ni5 Cast Aged Gunmetal Mechanical properties

Young’s modulus79–82GPa
Specific stiffness8.97–9.33MN.m/kg
Yield strength (elastic limit)280–320MPa
Tensile strength430–480MPa
Specific strength31.8–36.4kN.m/kg
Elongation3–5% strain
Compressive strength280–320MPa
Flexural modulus79–82GPa
Flexural strength (modulus of rupture)280–320MPa
Shear modulus29.2–30.3GPa
Bulk modulus85.3–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor20
Hardness – Vickers80–160HV
Elastic stored energy (springs)489–634kJ/m3
Fatigue strength at 10^7 cycles185–199MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
171–215MPa

CuSn7Zn2Ni5 Impact & fracture properties

Fracture toughness40.4–44.2MPa.m0.5
Toughness (G)20.3–24.3kJ/m2

CuSn7Zn2Ni5 Cast Aged Gunmetal Thermal properties

Melting point917–1040°C
Maximum service temperature97–110°C
Minimum service temperature-63–-48°C
Thermal conductivity63–65W/m.°C
Specific heat capacity383–384J/kg.°C
Thermal expansion coefficient17.5–18.5µstrain/°C
Thermal shock resistance192–223°C
Thermal distortion resistance3.45–3.67MW/m
Latent heat of fusion220–240kJ/kg

CuSn7Zn2Ni5 Electrical properties

Electrical resistivity14.5–15.8µohm.cm
Electrical conductivity10.9–11.9%IACS
Galvanic potential-0.24–-0.16V

CuSn7Zn2Ni5 Magnetic properties

Magnetic typeNon-magnetic

CuSn7Zn2Ni5 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2990–3050m/s
Mechanical loss coefficient (tan delta)3.9e-5–5.1e-5 

CuSn7Zn2Ni5 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed27.4 m/min
WeldabilityUnsuitable

CuSn7Zn2Ni5 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn7Zn2Ni5 Cast Aged Gunmetal Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

CuSn7Zn2Ni5 Notes

CuSn7Zn2Ni5 Cast Aged Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuSn7Zn2Ni5 Standards with similar compositions

USA: C94700 to ASTM B30
Tradenames: BELMONT NO. 48812, HOLFOS G 3-TF (FULLY HEAT TREATED), HOLFOS G3 (AS CAST), HOLFOS G3-WP, WRM 50N H.T.