Home » Gunmetal Alloys » CuSn10Zn2 (C90500) Admiralty Gunmetal, Cast Material Data Sheet
CuSn10Zn2 (C90500) Admiralty Gunmetal, Cast Material Data Sheet
CuSn10Zn2 (C90500) Admiralty Gunmetal Material Data Sheet (Cast)
C90500 Cast Gunmetal Overview
C90500 cast gunmetal is a cast gunmetal (UNS C90500), known as admiralty gunmetal. Condition: Cast. This C90500 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90500 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C90500 gunmetal castings with in-house CNC machining and inspects them before shipment.
C90500 Designation
CuSn10Zn2
UNS number
C90500
ISO name
CuSn10Zn2
GB (Chinese) name
CuSn10Zn2
JIS (Japanese) name
BC 3
C90500 Typical uses
Pumps and valves, bearings, valve guides, marine uses.
C90500 Cast Gunmetal Composition detail
Al (aluminum)
0
–
0.005
%
Cu (copper)
84.2
–
90
%
Fe (iron)
0
–
0.2
%
Ni (nickel)
0
–
1
%
P (phosphorus)
0
–
0.05
%
Pb (lead)
0
–
0.3
%
S (sulfur)
0
–
0.05
%
Sb (antimony)
0
–
0.2
%
Si (silicon)
0
–
0.005
%
Sn (tin)
9
–
11
%
Zn (zinc)
1
–
3
%
C90500 Physical properties
Density
8.75
–
8.85
g/cm3
C90500 Cast Gunmetal Mechanical properties
Young’s modulus
79
–
82
GPa
Specific stiffness
8.97
–
9.33
MN.m/kg
Yield strength (elastic limit)
130
–
170
MPa
Tensile strength
250
–
340
MPa
Specific strength
14.8
–
19.3
kN.m/kg
Elongation
5
–
16
% strain
Compressive strength
130
–
170
MPa
Flexural modulus
79
–
82
GPa
Flexural strength (modulus of rupture)
130
–
170
MPa
Shear modulus
29.2
–
30.3
GPa
Bulk modulus
85.3
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
70
–
95
HV
Elastic stored energy (springs)
107
–
177
kJ/m3
Fatigue strength at 10^7 cycles
130
–
159
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
106
–
195
MPa
C90500 Impact & fracture properties
Fracture toughness
59.4
–
67.9
MPa.m0.5
Toughness (G)
44
–
57.1
kJ/m2
C90500 Cast Gunmetal Thermal properties
Melting point
887
–
1040
°C
Maximum service temperature
200
–
210
°C
Minimum service temperature
-63
–
-48
°C
Thermal conductivity
62
–
64
W/m.°C
Specific heat capacity
383
–
384
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
89.5
–
118
°C
Thermal distortion resistance
3.39
–
3.61
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C90500 Electrical properties
Electrical resistivity
15.8
–
17.4
µohm.cm
Electrical conductivity
9.91
–
10.9
%IACS
Galvanic potential
-0.24
–
-0.16
V
C90500 Magnetic properties
Magnetic type
Non-magnetic
C90500 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2990
–
3050
m/s
Mechanical loss coefficient (tan delta)
1.38e-4
–
2.37e-4
C90500 Processing properties
Metal casting
Acceptable
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
39.6 m/min
Weldability
Unsuitable
C90500 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
C90500 Cast Gunmetal Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C90500 Notes
C90500 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C90500 Standards with similar compositions
Czech Republic: CuSn10Zn2 to CSN 423138
Germany: 2.1086 to DIN, 2.1087 to DIN 17656, GB-CuSn10Zn to DIN 17656, G-CuSn10Zn to DIN
Japan: CAC403 to JIS H5120, CAC403C to JIS H5121
Norway: 16512 to NS 16512
USA: C90500, C90500 to AMS 4845, C90500 to ASTM B22, C90500 to ASTM B271, C90500 to ASTM B30, C90500 to ASTM B584, C90500 to ASTM B763, C90500 to QQ C-390, C90500 to SAE J462, UNS C90500