CuPb5Sn5Zn5 (85-5-5-5) (C83600) Leaded Gunmetal, Cast Material Data Sheet

CuPb5Sn5Zn5 (85-5-5-5) (C83600) Leaded Gunmetal Material Data Sheet (Cast)

C83600 Cast Gunmetal Overview

C83600 cast gunmetal is a cast gunmetal (UNS C83600, EN CC491K), known as leaded gunmetal. Condition: Cast. This C83600 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C83600 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C83600 gunmetal castings with in-house CNC machining and inspects them before shipment.

C83600 Designation

CuPb5Sn5Zn5 (85-5-5-5)
UNS numberC83600
EN nameCC491K
ISO nameCuPb5Sn5Zn5
JIS (Japanese) nameBC 6 / BC ln 6

C83600 Typical uses

Pumps, valves, housings to resist corrosion, low-stressed bushings.

C83600 Cast Gunmetal Composition detail

Al (aluminum)0–0.005%
Cu (copper)80.3–88%
Fe (iron)0–0.3%
Ni (nickel)0–1%
P (phosphorus)0–0.05%
Pb (lead)4–6%
S (sulfur)0–0.08%
Sb (antimony)0–0.25%
Si (silicon)0–0.005%
Sn (tin)4–6%
Zn (zinc)4–6%

C83600 Physical properties

Density8.75–8.85g/cm3

C83600 Cast Gunmetal Mechanical properties

Young’s modulus79–82GPa
Specific stiffness8.97–9.33MN.m/kg
Yield strength (elastic limit)110–140MPa
Tensile strength200–280MPa
Specific strength12.5–15.9kN.m/kg
Elongation6–15% strain
Compressive strength110–140MPa
Flexural modulus79–82GPa
Flexural strength (modulus of rupture)110–140MPa
Shear modulus29.2–30.3GPa
Bulk modulus85.3–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers80–95HV
Elastic stored energy (springs)76.1–120kJ/m3
Fatigue strength at 10^7 cycles113–140MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
90.6–175MPa

C83600 Impact & fracture properties

Fracture toughness65.5–73.1MPa.m0.5
Toughness (G)53.4–66.3kJ/m2

C83600 Cast Gunmetal Thermal properties

Melting point927–1050°C
Maximum service temperature180–190°C
Minimum service temperature-63–-48°C
Thermal conductivity70–75W/m.°C
Specific heat capacity383–384J/kg.°C
Thermal expansion coefficient17.5–18.5µstrain/°C
Thermal shock resistance75.7–97°C
Thermal distortion resistance3.85–4.21MW/m
Latent heat of fusion220–240kJ/kg

C83600 Electrical properties

Electrical resistivity11.5–17.4µohm.cm
Electrical conductivity9.91–15%IACS
Galvanic potential-0.25–-0.17V

C83600 Magnetic properties

Magnetic typeNon-magnetic

C83600 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2990–3050m/s
Mechanical loss coefficient (tan delta)2.04e-4–3.31e-4 

C83600 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed79.2 m/min
WeldabilityUnsuitable

C83600 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

C83600 Cast Gunmetal Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible

C83600 Notes

C83600 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C83600 Standards with similar compositions

Australia: C83600A to AS 2738
Czech Republic: CuSn5PbZn5 to CSN 423135
Europe: CB491K to CEN EN 1982, CC491K to CEN EN 1982
Germany: 2.1096 to DIN, G-CuSn5ZnPb to DIN
International: CuPb5Sn5Zn5 to ISO 4382-1
Japan: CAC406 to JIS H5120, CAC406C to JIS H5121
Norway: 16530 to NS 16530
USA: C83600, C83600 to ASTM B271, C83600 to ASTM B30, C83600 to ASTM B584, C83600 to ASTM B62, UNS C83600
Venezuela: C83600 to COPANT 801
Tradenames: AMPCOLOY 74, CRANE STEAM BRONZE, FEDERALOY F-3, LILY BRAND NO. 4, MODIFIED OUNCE METAL, PROMET 85A, WRM 55