AISI 1144 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 1144 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 1144 Oil Quenched & Tempered at 205°C Overview

AISI 1144 oil quenched tempered 205°C is AISI 1144 resulfurized medium carbon steel (UNS G11440) in the oil quenched & tempered at 205°C condition. This AISI 1144 oil quenched tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1144 conditions in our AISI 1144 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1144 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1144 steel parts in-house and inspects them before shipment.

AISI 1144 Oil Quenched & Tempered at 205°C Designation

AISI 1144
ConditionTempered at 205°C & oil quenched
UNS numberG11440
US nameASTM G11440, ASTM 1144 Class B, ASTM 1144 Class A, ASTM 1144
GB (Chinese) name~Y40Mn
JIS (Japanese) nameSUM43

AISI 1144 Oil Quenched & Tempered at 205°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1144 Oil Quenched & Tempered at 205°C Composition detail

C (carbon)0.4–0.48%
Fe (iron)97.5–98%
Mn (manganese)1.35–1.65%
P (phosphorus)0–0.04%
S (sulfur)0.24–0.33%

AISI 1144 Oil Quenched & Tempered at 205°C Physical properties

Density7.8–7.9g/cm3

AISI 1144 Oil Quenched & Tempered at 205°C Mechanical properties

Young’s modulus200–215GPa
Specific stiffness25.5–27.4MN.m/kg
Yield strength (elastic limit)560–695MPa
Tensile strength780–970MPa
Specific strength71.3–88.6kN.m/kg
Elongation13–21% strain
Compressive strength560–695MPa
Flexural modulus200–215GPa
Flexural strength (modulus of rupture)560–695MPa
Shear modulus77–84GPa
Bulk modulus155–175GPa
Poisson’s ratio0.285–0.295 
Shape factor39
Hardness – Vickers255–305HV
Elastic stored energy (springs)762–1160kJ/m3
Fatigue strength at 10^7 cycles359–420MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
311–485MPa

AISI 1144 Oil Quenched & Tempered at 205°C Impact & fracture properties

Fracture toughness36–61MPa.m0.5
Toughness (G)6.6–17kJ/m2

AISI 1144 Oil Quenched & Tempered at 205°C Thermal properties

Melting point1420–1500°C
Maximum service temperature165–195°C
Minimum service temperature-48–-18°C
Thermal conductivity47–53W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient12.5–14µstrain/°C
Thermal shock resistance201–258°C
Thermal distortion resistance3.48–4.09MW/m
Latent heat of fusion270–275kJ/kg

AISI 1144 Oil Quenched & Tempered at 205°C Electrical properties

Electrical resistivity16–20µohm.cm
Electrical conductivity8.62–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1144 Oil Quenched & Tempered at 205°C Magnetic properties

Magnetic typeMagnetic

AISI 1144 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5240m/s
Mechanical loss coefficient (tan delta)5.1e-4–6.4e-4 

AISI 1144 Oil Quenched & Tempered at 205°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed27.1 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency0.625 – 0.755

AISI 1144 Oil Quenched & Tempered at 205°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1144 Oil Quenched & Tempered at 205°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1144 Oil Quenched & Tempered at 205°C Standards with similar compositions

Australia: 1144 to AS 1442, 1144 to AS 1443
Italy: CF44SMn28 to UNI 4838, CF44SMnPb28 to UNI 4838
Japan: SUM43 to JIS G4804
Mexico: 1144 to NMX-B-301
Pan America: 1444 to COPANT 330, 1444 to COPANT 331, 1444 to COPANT 332
Russia: AS45G2 to GOST 1414
UK: 226M44 to BS 970/3, 44SMn28 to BS EN 10277-3, 44SMnPb28 to BS EN 10277-3
USA: 1144, 1144 Class A to ASTM A311/A311M, 1144 Class B to ASTM A311/A311M, 1144 to ASTM A29/A29M, 1144 to ASTM A519, 1144 to SAE J403, 11L44, C1144 to FED QQ-S-637A, G11440 to ASTM A510/A510M, G11440 to ASTM A576-90b, UNS G11440
Tradenames: C1144 MOD, ELASTUF STRAINFREE, JALCASE 10, JALCASE 100, JALCASE 9, LASALLE 1144, RYTENSE 44, S-1144, SAARSTAHL SAE 1144, STRAIN TEMPERED 1144, STRESS-PROOF NO. 1, STRESS-PROOF NO. 2, STRESS-PROOF NO. 3, WYCO 100-44, WYCO 125-44