AISI 1137 Water Quenched & Tempered at 650°C Material Data Sheet
AISI 1137 Water Quenched & Tempered at 650°C Material Data Sheet
AISI 1137 Water Quenched & Tempered at 650°C Overview
AISI 1137 water quenched tempered 650°C is AISI 1137 resulfurized medium carbon steel (UNS G11370) in the water quenched & tempered at 650°C condition. This AISI 1137 water quenched tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1137 conditions in our AISI 1137 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1137 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1137 steel parts in-house and inspects them before shipment.
AISI 1137 Water Quenched & Tempered at 650°C Designation
AISI 1137
Condition
Tempered at 650°C & water quenched
UNS number
G11370
US name
ASTM G11370, ASTM 1137 Class A, ASTM 1137, AMS 5024, ~SAE 1138
JIS (Japanese) name
SUM41
AISI 1137 Water Quenched & Tempered at 650°C Typical uses
Heavy duty shafts, axles, crankshafts, couplings, used particularly where enhanced machinability is important.
AISI 1137 Water Quenched & Tempered at 650°C Composition detail
C (carbon)
0.32
–
0.39
%
Fe (iron)
97.8
–
98.2
%
Mn (manganese)
1.35
–
1.65
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0.08
–
0.13
%
AISI 1137 Water Quenched & Tempered at 650°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 1137 Water Quenched & Tempered at 650°C Mechanical properties
Young’s modulus
200
–
215
GPa
Specific stiffness
25.5
–
27.4
MN.m/kg
Yield strength (elastic limit)
475
–
590
MPa
Tensile strength
580
–
715
MPa
Specific strength
60.5
–
75.2
kN.m/kg
Elongation
20
–
30
% strain
Compressive strength
475
–
590
MPa
Flexural modulus
200
–
215
GPa
Flexural strength (modulus of rupture)
475
–
590
MPa
Shear modulus
77
–
84
GPa
Bulk modulus
155
–
175
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
45
Hardness – Vickers
173
–
213
HV
Elastic stored energy (springs)
549
–
832
kJ/m3
Fatigue strength at 10^7 cycles
292
–
339
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
254
–
390
MPa
AISI 1137 Water Quenched & Tempered at 650°C Impact & fracture properties
Fracture toughness
33
–
55
MPa.m0.5
Toughness (G)
5.53
–
13.9
kJ/m2
AISI 1137 Water Quenched & Tempered at 650°C Thermal properties
Melting point
1440
–
1510
°C
Maximum service temperature
327
–
352
°C
Minimum service temperature
-58
–
-33
°C
Thermal conductivity
47
–
53
W/m.°C
Specific heat capacity
440
–
500
J/kg.°C
Thermal expansion coefficient
12
–
13.5
µstrain/°C
Thermal shock resistance
177
–
228
°C
Thermal distortion resistance
3.61
–
4.26
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 1137 Water Quenched & Tempered at 650°C Electrical properties
Electrical resistivity
16
–
19
µohm.cm
Electrical conductivity
9.07
–
10.8
%IACS
Galvanic potential
-0.52
–
-0.44
V
AISI 1137 Water Quenched & Tempered at 650°C Magnetic properties
Magnetic type
Magnetic
AISI 1137 Water Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5050
–
5240
m/s
Mechanical loss coefficient (tan delta)
6.4e-4
–
8.1e-4
AISI 1137 Water Quenched & Tempered at 650°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
33.5 m/min
Weldability Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency
0.545 – 0.665
AISI 1137 Water Quenched & Tempered at 650°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 1137 Water Quenched & Tempered at 650°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible
AISI 1137 Water Quenched & Tempered at 650°C Notes
AISI 1137 Water Quenched & Tempered at 650°C Warning
Free cutting’ steel – in common with all such steels, it is not recommended where welding is involved.
AISI 1137 Water Quenched & Tempered at 650°C Other notes
A free-cutting version of AISI 1040 grade, used when enhanced machinability is required.
AISI 1137 Water Quenched & Tempered at 650°C Standards with similar compositions
Australia: K1137 to AS 1442
Canada: X46 to CSA B193, X52 to CSA B193
Italy: 35SMn10 to UNI 4838, CF35SMn10 to UNI 4838, CF35SMnPb10 to UNI 4838
Japan: SUM41 to JIS G4804
Mexico: 1132 to NMX-B-301, 1137 to NMX-B-301
Pan America: 1137 to COPANT 330, 1137 to COPANT 331, 1137 to COPANT 332, 1137 to COPANT 514
UK: 36SMn14 to BS EN 10277-3, 36SMnPb14 to BS EN 10277-3
USA: 1132, 1132 to ASTM A29/A29M, 1132 to ASTM A519, 1132 to SAE J403, 1137, 1137 Class A to ASTM A311/A311M, 1137 to ASTM A29/A29M, 1137 to ASTM A519, 1137 to FED QQ-S-633A, 1137 to SAE J403, 5024 to AMS 5024F, G11320 to ASTM A510/A510M, G11320 to ASTM A576-90b, G11370 to ASTM A510/A510M, G11370 to ASTM A576-90b, MIL-S-16124 to MIL-S-16124, UNS G11320, UNS G11370, UNS G11374