AISI 1118 Annealed Material Data Sheet

AISI 1118 Annealed Material Data Sheet

AISI 1118 Annealed Overview

AISI 1118 annealed is AISI 1118 resulfurized low carbon steel (UNS G11180) in the annealed condition. This AISI 1118 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1118 conditions in our AISI 1118 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1118 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1118 steel parts in-house and inspects them before shipment.

AISI 1118 Annealed Designation

AISI 1118
ConditionAnnealed
UNS numberG11180
US nameASTM G11180, ASTM 11L18, ASTM 1118, ~ASTM D

AISI 1118 Annealed Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1118 Annealed Composition detail

C (carbon)0.14–0.2%
Fe (iron)98–98.5%
Mn (manganese)1.3–1.6%
P (phosphorus)0–0.04%
S (sulfur)0.08–0.13%

AISI 1118 Annealed Physical properties

Density7.8–7.9g/cm3

AISI 1118 Annealed Mechanical properties

Young’s modulus205–215GPa
Specific stiffness26.1–27.4MN.m/kg
Yield strength (elastic limit)255–315MPa
Tensile strength405–495MPa
Specific strength32.5–40.1kN.m/kg
Elongation27–42% strain
Compressive strength255–315MPa
Flexural modulus205–215GPa
Flexural strength (modulus of rupture)255–315MPa
Shear modulus79–84GPa
Bulk modulus158–175GPa
Poisson’s ratio0.285–0.295 
Shape factor62
Hardness – Vickers128–150HV
Elastic stored energy (springs)156–234kJ/m3
Fatigue strength at 10^7 cycles227–262MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
197–302MPa

AISI 1118 Annealed Impact & fracture properties

Fracture toughness50–79MPa.m0.5
Toughness (G)12.4–28.5kJ/m2

AISI 1118 Annealed Thermal properties

Melting point1490–1530°C
Maximum service temperature343–357°C
Minimum service temperature-68–-38°C
Thermal conductivity49–54W/m.°C
Specific heat capacity460–500J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance97.7–125°C
Thermal distortion resistance3.89–4.55MW/m
Latent heat of fusion270–275kJ/kg

AISI 1118 Annealed Electrical properties

Electrical resistivity15–20µohm.cm
Electrical conductivity8.62–11.5%IACS
Galvanic potential-0.52–-0.44V

AISI 1118 Annealed Magnetic properties

Magnetic typeMagnetic

AISI 1118 Annealed Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5240m/s
Mechanical loss coefficient (tan delta)0.00106–0.00131 

AISI 1118 Annealed Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed45.7 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency0.357 – 0.467

AISI 1118 Annealed Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1118 Annealed Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1118 Annealed Standards with similar compositions

Argentina: IRAM 1118 to IAS
Canada: C1118 to CSA 95-1/1
India: 20Mn2 to IS 6967
Mexico: 1118 to NMX-B-301
Pan America: 1024 to COPANT 333, 1118 to COPANT 330, 1118 to COPANT 331, 1118 to COPANT 514
UK: 174H20 to BS 970/1, 175H23 to BS 970/1
USA: 1118, 1118 to ASTM A29/A29M, 1118 to ASTM A519, 1118 to FED QQ-S-00643, 1118 to FED QQ-S-633A, 1118 to SAE J403, 11L18 to ASTM A519, C1118 to FED QQ-S-637A, G11180 to ASTM A510/A510M, G11180 to ASTM A576-90b, MIL-S-16124 to MIL-S-16124, MIL-S-16611 to MIL-S-16611, UNS G11180
Tradenames: AMERCUT C-1118, B&W 1118FM, C.M.S., JESSOP AM-2S, NATIONAL TUBE C-1118, S-1118