AISI 1095 Water Quenched & Tempered at 425°C Material Data Sheet
AISI 1095 Water Quenched & Tempered at 425°C Overview
| AISI 1095 water quenched tempered 425°C is AISI 1095 high carbon steel (UNS G10950) in the water quenched & tempered at 425°C condition. This AISI 1095 water quenched tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1095 conditions in our AISI 1095 yield, tensile and hardness comparison. Looking for AISI 1095 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1095 steel parts in-house and inspects them before shipment. |
AISI 1095 Water Quenched & Tempered at 425°C Designation
| AISI 1095 | |
| Condition | Tempered at 425°C & water quenched |
| UNS number | G10950 |
| US name | ASTM 1095, ASME G10950 |
| EN name | ~HS95 |
AISI 1095 Water Quenched & Tempered at 425°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1095 Water Quenched & Tempered at 425°C Composition detail
| C (carbon) | 0.9 | – | 1.03 | % |
| Fe (iron) | 98.4 | – | 98.8 | % |
| Mn (manganese) | 0.3 | – | 0.5 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1095 Water Quenched & Tempered at 425°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1095 Water Quenched & Tempered at 425°C Mechanical properties
| Young’s modulus | 200 | – | 215 | GPa |
| Specific stiffness | 25.5 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 855 | – | 1060 | MPa |
| Tensile strength | 1230 | – | 1520 | MPa |
| Specific strength | 109 | – | 135 | kN.m/kg |
| Elongation | 10.5 | – | 15.5 | % strain |
| Compressive strength | 855 | – | 1060 | MPa |
| Flexural modulus | 200 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 855 | – | 1060 | MPa |
| Shear modulus | 77 | – | 84 | GPa |
| Bulk modulus | 155 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 26 | |||
| Hardness – Vickers | 360 | – | 430 | HV |
| Elastic stored energy (springs) | 1780 | – | 2690 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 494 | – | 573 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 431 | – | 657 | MPa |
AISI 1095 Water Quenched & Tempered at 425°C Impact & fracture properties
| Fracture toughness | 30 | – | 53 | MPa.m0.5 |
| Toughness (G) | 4.62 | – | 12.7 | kJ/m2 |
AISI 1095 Water Quenched & Tempered at 425°C Thermal properties
| Melting point | 1290 | – | 1470 | °C |
| Maximum service temperature | 273 | – | 336 | °C |
| Minimum service temperature | -28 | – | 2 | °C |
| Thermal conductivity | 47 | – | 52 | W/m.°C |
| Specific heat capacity | 440 | – | 480 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13.5 | µstrain/°C |
| Thermal shock resistance | 325 | – | 437 | °C |
| Thermal distortion resistance | 3.62 | – | 4.54 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1095 Water Quenched & Tempered at 425°C Electrical properties
| Electrical resistivity | 17 | – | 20 | µohm.cm |
| Electrical conductivity | 8.62 | – | 10.1 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 1095 Water Quenched & Tempered at 425°C Magnetic properties
| Magnetic type | Magnetic |
AISI 1095 Water Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5050 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 3.3e-4 | – | 4.1e-4 | |
AISI 1095 Water Quenched & Tempered at 425°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Limited use |
| Metal hot forming | Limited use |
| Metal press forming | Acceptable |
| Metal deep drawing | Limited use |
| Machining speed | 11.3 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.95 – 1.11 |
AISI 1095 Water Quenched & Tempered at 425°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1095 Water Quenched & Tempered at 425°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Slightly susceptible |
AISI 1095 Water Quenched & Tempered at 425°C Standards with similar compositions
| Mexico: 1086 to NMX-B-301, 1095 to NMX-B-301 |
| Pan America: 1095 to COPANT 330, 1095 to COPANT 331 |
| UK: 060A96 to BS 970/1 |
| USA: 1086, 1086 to ASTM A29/A29M, 1086 to ASTM A568/A568M, 1086 to ASTM A713, 1086 to SAE J1249, 1086 to SAE J403, 1095, 1095 to ASTM A29/A29M, 1095 to ASTM A568/A568M, 1095 to ASTM A713, 1095 to MIL-S-7947A, 1095 to SAE J403, 7304 to AMS 7304, C10 to MIL-S-16788A, C1095 to FED QQ-S-700D, G10860 to ASTM A510/A510M, G10950 to ASTM A510/A510M, G10950 to ASTM A576-90b, UNS G10860, UNS G10860 to UNS, UNS G10950, UNS G10950 to UNS |
| Tradenames: ACHORN STANDARD CARBON, AIRCO NO. 85, AQUATOUGH 100, ATLAS REFINED-10, BEST, CARR’S QUALITY RED LABEL, CHANNELER, COPPCO EXTRA, CORINTH, DISSTON NO. 5190, EIS-V3, ELECTREX, FAGERSTA OVERCOAT AXE, FAGERSTA REGULAR, FAGERSTA SPECIAL, FIRTH-BROWN F95C, FORTUNA GSB10, FORTUNA W93, G.W. REGULAR, G.W. SPECIAL, H S C COLD HEADER, H S C REGULAR, JESSOP BLUE LABEL, JESSOP SHEET SPRING, K.E.A. 108, MARREL MO, MCINNES FOLDIER DIE, PAGE HIGH CARBON, PREMIER HC WELD, RED SEAL DIE STEEL, S/100, SAVILLE BEST CAST STEEL, SAVILLE CAST, SAVILLE CAST STEEL WARRANTED, SOLID DRILL, SPRING STEEL, STANDARD, TRU-COR DRILL ROD, TULIPE EXTRA NO. 3, UNA NO. 325, WHELCO STD |