AISI 1050 Water Quenched & Tempered at 315°C Material Data Sheet
AISI 1050 Water Quenched & Tempered at 315°C Overview
| AISI 1050 water quenched tempered 315°C is AISI 1050 medium carbon steel (UNS G10500) in the water quenched & tempered at 315°C condition. This AISI 1050 water quenched tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1050 conditions in our AISI 1050 yield, tensile and hardness comparison. Looking for AISI 1050 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1050 steel parts in-house and inspects them before shipment. |
AISI 1050 Water Quenched & Tempered at 315°C Designation
| AISI 1050 | |
| Condition | Tempered at 315°C & water quenched |
| UNS number | G10500 |
| US name | ASTM 1050 Class B, ASTM 1050 Class A, ASTM 1050, ASME G10530, ASME G10500, ASME G10490, ~ASME 1053, ~ASME 1049 |
| EN name | ~HS50, ~Ck53 |
| JIS (Japanese) name | ~STKM17C, ~STKM17A |
AISI 1050 Water Quenched & Tempered at 315°C Typical uses
| Sprockets, cams, crankshafts, small gears, machine tools, rifle barrels, hammers, machine parts requiring reasonable strength and wear resistance but where toughness is not so important. |
AISI 1050 Water Quenched & Tempered at 315°C Composition detail
| C (carbon) | 0.48 | – | 0.55 | % |
| Fe (iron) | 98.5 | – | 98.9 | % |
| Mn (manganese) | 0.6 | – | 0.9 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1050 Water Quenched & Tempered at 315°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1050 Water Quenched & Tempered at 315°C Mechanical properties
| Young’s modulus | 208 | – | 216 | GPa |
| Specific stiffness | 26.5 | – | 27.5 | MN.m/kg |
| Yield strength (elastic limit) | 710 | – | 875 | MPa |
| Tensile strength | 980 | – | 1200 | MPa |
| Specific strength | 90.4 | – | 111 | kN.m/kg |
| Elongation | 10 | – | 16 | % strain |
| Compressive strength | 710 | – | 875 | MPa |
| Flexural modulus | 208 | – | 216 | GPa |
| Flexural strength (modulus of rupture) | 710 | – | 875 | MPa |
| Shear modulus | 80 | – | 85 | GPa |
| Bulk modulus | 161 | – | 176 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 32 | |||
| Hardness – Vickers | 400 | – | 490 | HV |
| Elastic stored energy (springs) | 1200 | – | 1790 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 422 | – | 487 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 369 | – | 557 | MPa |
AISI 1050 Water Quenched & Tempered at 315°C Impact & fracture properties
| Fracture toughness | 32 | – | 55 | MPa.m0.5 |
| Toughness (G) | 5.12 | – | 13.5 | kJ/m2 |
AISI 1050 Water Quenched & Tempered at 315°C Thermal properties
| Melting point | 1400 | – | 1500 | °C |
| Maximum service temperature | 275 | – | 305 | °C |
| Minimum service temperature | -38 | – | -8 | °C |
| Thermal conductivity | 49 | – | 53 | W/m.°C |
| Specific heat capacity | 465 | – | 505 | J/kg.°C |
| Thermal expansion coefficient | 10 | – | 12 | µstrain/°C |
| Thermal shock resistance | 296 | – | 389 | °C |
| Thermal distortion resistance | 4.22 | – | 5.13 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1050 Water Quenched & Tempered at 315°C Electrical properties
| Electrical resistivity | 16 | – | 19 | µohm.cm |
| Electrical conductivity | 9.07 | – | 10.8 | %IACS |
| Galvanic potential | -0.52 | – | -0.44 | V |
AISI 1050 Water Quenched & Tempered at 315°C Magnetic properties
| Magnetic type | Magnetic |
AISI 1050 Water Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5140 | – | 5250 | m/s |
| Mechanical loss coefficient (tan delta) | 4e-4 | – | 5.1e-4 | |
AISI 1050 Water Quenched & Tempered at 315°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Acceptable |
| Metal press forming | Acceptable |
| Metal deep drawing | Acceptable |
| Machining speed | 12.2 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.58 – 0.7 |
AISI 1050 Water Quenched & Tempered at 315°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1050 Water Quenched & Tempered at 315°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Slightly susceptible |
AISI 1050 Water Quenched & Tempered at 315°C Notes
| AISI 1050 Water Quenched & Tempered at 315°C Other notes |
| Can be flame or induction hardened to give high levels of wear resistance. |
AISI 1050 Water Quenched & Tempered at 315°C Standards with similar compositions
| India: 50C8 to IS 1570/2/1, 55C8 to IS 1570/2/1, C55Mn75 to IS 1570/2/1, CDS-5 to IS 3074, T50 to IS 3749 |
| Mexico: 1045 to NMX-B-203-SCFI, 1045 to NMX-B-301, 1046 to NMX-B-301, 1049 to NMX-B-301, 1050 to NMX-B-203-SCFI, 1050 to NMX-B-301, 1053 to NMX-B-301, 1055 to NMX-B-301 |
| Pan America: 1045 to COPANT 330, 1045 to COPANT 331, 1045 to COPANT 333, 1050 to COPANT 330, 1050 to COPANT 331, 1050 to COPANT 333, 1055 to COPANT 330, 1055 to COPANT 331, 1055 to COPANT 333 |
| UK: 060A52 to BS 970/1, 070M55 to BS 970/1, 080A52 to BS 970/1, 080H46 to BS 970/1, 080M46 to BS 970/1 |
| USA: 1045, 1045 Class A to ASTM A311/A311M, 1045 Class B to ASTM A311/A311M, 1045 to ASTM A29/A29M, 1045 to ASTM A519, 1045 to ASTM A568/A568M, 1045 to FED QQ-S-700D, 1045 to FED QQ-W-461H, 1045 to SAE J403, 1046, 1046 to ASTM A29/A29M, 1046 to SAE J403, 1049, 1049 to ASTM A29/A29M, 1049 to ASTM A568/A568M, 1049 to SAE J403, 1050, 1050 Class A to ASTM A311/A311M, 1050 Class B to ASTM A311/A311M, 1050 to ASTM A29/A29M, 1050 to ASTM A513, 1050 to ASTM A519, 1050 to ASTM A568/A568M, 1050 to DoD-F-24669/1, 1050 to MIL-S-16974E, 1050 to SAE J403, 1053, 1053 to ASTM A29/A29M, 1053 to SAE J403, 1055, 1055 to ASTM A29/A29M, 1055 to ASTM A713, 1055 to SAE J403, 10L45, 10L50, 1553, C1045 to FED QQ-S-635B, C1050 to FED QQ-S-635B, C1050 to FED QQ-S-700D, C1055 to FED QQ-S-700D, C5 to MIL-S-16788A, G10450 to ASTM A510/A510M, G10450 to ASTM A576-90b, G10460 to ASTM A510/A510M, G10460 to ASTM A576-90b, G10490 to ASTM A510/A510M, G10490 to ASTM A576-90b, G10500 to ASTM A510/A510M, G10500 to ASTM A576-90b, G10500 to MIL-S-46059, G10530 to ASTM A510/A510M, G10530 to ASTM A576-90b, G10550 to ASTM A510/A510M, G10550 to ASTM A576-90b, UNS G10450, UNS G10450 to UNS, UNS G10460, UNS G10490, UNS G10500, UNS G10530, UNS G10550, UNS G15530, UNS K04700 |
| Tradenames: ASCOMETAL 51S7, ASCOMETAL XC55H1-H2, B.S.C. A-31, B/55, BOHLER WB, CARR’S QUALITY P 256, DYNAMIC C-1-6, HARDFLEX-11, HI-QUA-LED 10L50, INGERSOLL I-50, LASALLE 1045, MARREL M3, RED DIAMOND 9H, SECO XXX, SIMONDS 1050 ROTARY RULE, STRAIN TEMPERED 1050, TULIPE EXTRA NO. 6, WITTEN W 50 E, WYCO 100-50 |