AISI 1050 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1050 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1050 Oil Quenched & Tempered at 425°C Overview

AISI 1050 oil quenched tempered 425°C is AISI 1050 medium carbon steel (UNS G10500) in the oil quenched & tempered at 425°C condition. This AISI 1050 oil quenched tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1050 conditions in our AISI 1050 yield, tensile and hardness comparison. Looking for AISI 1050 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1050 steel parts in-house and inspects them before shipment.

AISI 1050 Oil Quenched & Tempered at 425°C Designation

AISI 1050
ConditionTempered at 425°C & oil quenched
UNS numberG10500
US nameASTM 1050 Class B, ASTM 1050 Class A, ASTM 1050, ASME G10530, ASME G10500, ASME G10490, ~ASME 1053, ~ASME 1049
EN name~HS50, ~Ck53
JIS (Japanese) name~STKM17C, ~STKM17A

AISI 1050 Oil Quenched & Tempered at 425°C Typical uses

Sprockets, cams, crankshafts, small gears, machine tools, rifle barrels, hammers, machine parts requiring reasonable strength and wear resistance but where toughness is not so important.

AISI 1050 Oil Quenched & Tempered at 425°C Composition detail

C (carbon)0.48–0.55%
Fe (iron)98.5–98.9%
Mn (manganese)0.6–0.9%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1050 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 1050 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)585–720MPa
Tensile strength840–1040MPa
Specific strength74.5–91.7kN.m/kg
Elongation16–24% strain
Compressive strength585–720MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)585–720MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor39
Hardness – Vickers250–310HV
Elastic stored energy (springs)815–1210kJ/m3
Fatigue strength at 10^7 cycles378–439MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
329–504MPa

AISI 1050 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness37–61MPa.m0.5
Toughness (G)6.79–16.7kJ/m2

AISI 1050 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1400–1500°C
Maximum service temperature313–347°C
Minimum service temperature-48–-18°C
Thermal conductivity49–53W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient10–12µstrain/°C
Thermal shock resistance244–320°C
Thermal distortion resistance4.22–5.13MW/m
Latent heat of fusion270–275kJ/kg

AISI 1050 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity16–19µohm.cm
Electrical conductivity9.07–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1050 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 1050 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5140–5250m/s
Mechanical loss coefficient (tan delta)4.8e-4–6e-4 

AISI 1050 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed17.7 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.58 – 0.7

AISI 1050 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1050 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1050 Oil Quenched & Tempered at 425°C Notes

AISI 1050 Oil Quenched & Tempered at 425°C Other notes
Can be flame or induction hardened to give high levels of wear resistance.

AISI 1050 Oil Quenched & Tempered at 425°C Standards with similar compositions

India: 50C8 to IS 1570/2/1, 55C8 to IS 1570/2/1, C55Mn75 to IS 1570/2/1, CDS-5 to IS 3074, T50 to IS 3749
Mexico: 1045 to NMX-B-203-SCFI, 1045 to NMX-B-301, 1046 to NMX-B-301, 1049 to NMX-B-301, 1050 to NMX-B-203-SCFI, 1050 to NMX-B-301, 1053 to NMX-B-301, 1055 to NMX-B-301
Pan America: 1045 to COPANT 330, 1045 to COPANT 331, 1045 to COPANT 333, 1050 to COPANT 330, 1050 to COPANT 331, 1050 to COPANT 333, 1055 to COPANT 330, 1055 to COPANT 331, 1055 to COPANT 333
UK: 060A52 to BS 970/1, 070M55 to BS 970/1, 080A52 to BS 970/1, 080H46 to BS 970/1, 080M46 to BS 970/1
USA: 1045, 1045 Class A to ASTM A311/A311M, 1045 Class B to ASTM A311/A311M, 1045 to ASTM A29/A29M, 1045 to ASTM A519, 1045 to ASTM A568/A568M, 1045 to FED QQ-S-700D, 1045 to FED QQ-W-461H, 1045 to SAE J403, 1046, 1046 to ASTM A29/A29M, 1046 to SAE J403, 1049, 1049 to ASTM A29/A29M, 1049 to ASTM A568/A568M, 1049 to SAE J403, 1050, 1050 Class A to ASTM A311/A311M, 1050 Class B to ASTM A311/A311M, 1050 to ASTM A29/A29M, 1050 to ASTM A513, 1050 to ASTM A519, 1050 to ASTM A568/A568M, 1050 to DoD-F-24669/1, 1050 to MIL-S-16974E, 1050 to SAE J403, 1053, 1053 to ASTM A29/A29M, 1053 to SAE J403, 1055, 1055 to ASTM A29/A29M, 1055 to ASTM A713, 1055 to SAE J403, 10L45, 10L50, 1553, C1045 to FED QQ-S-635B, C1050 to FED QQ-S-635B, C1050 to FED QQ-S-700D, C1055 to FED QQ-S-700D, C5 to MIL-S-16788A, G10450 to ASTM A510/A510M, G10450 to ASTM A576-90b, G10460 to ASTM A510/A510M, G10460 to ASTM A576-90b, G10490 to ASTM A510/A510M, G10490 to ASTM A576-90b, G10500 to ASTM A510/A510M, G10500 to ASTM A576-90b, G10500 to MIL-S-46059, G10530 to ASTM A510/A510M, G10530 to ASTM A576-90b, G10550 to ASTM A510/A510M, G10550 to ASTM A576-90b, UNS G10450, UNS G10450 to UNS, UNS G10460, UNS G10490, UNS G10500, UNS G10530, UNS G10550, UNS G15530, UNS K04700
Tradenames: ASCOMETAL 51S7, ASCOMETAL XC55H1-H2, B.S.C. A-31, B/55, BOHLER WB, CARR’S QUALITY P 256, DYNAMIC C-1-6, HARDFLEX-11, HI-QUA-LED 10L50, INGERSOLL I-50, LASALLE 1045, MARREL M3, RED DIAMOND 9H, SECO XXX, SIMONDS 1050 ROTARY RULE, STRAIN TEMPERED 1050, TULIPE EXTRA NO. 6, WITTEN W 50 E, WYCO 100-50