AISI 1010 Annealed Material Data Sheet
AISI 1010 Annealed Overview
| AISI 1010 annealed is AISI 1010 low carbon steel (UNS G10100) in the annealed condition. This AISI 1010 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for AISI 1010 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1010 steel parts in-house and inspects them before shipment. |
AISI 1010 Annealed Designation
| Carbon steel: AISI 1010 (annealed) | |
| Condition | Annealed |
| UNS number | G10100 |
| US name | SAE J527, ASTM MT 1010, ASTM M1012, ASTM M1010, ASTM 130, ASTM 1012, ASTM 1010, ASME G10120, ASME G10100, ~SAE SAE J526, ~ASTM M1008, ~ASTM G10130, ~AMS 5053 |
| EN name | HS12, ~HS4, ~ERW101, ~DC03, ~DC01 |
| EN number | ~1.1207, ~1.1121, ~1.0357, ~1.0347, ~1.0330 |
| ISO name | CC8X, CC8A, CC11X, CC11A, ~HR1, ~CR2, ~CE10 |
| GB (Chinese) name | ML10Al, ML08Al, ~Q215, ~CRB550 |
| JIS (Japanese) name | SGD 2, ~SPCC, ~SGD 1, ~SBC 300 |
AISI 1010 Annealed Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1010 Annealed Composition detail
| C (carbon) | 0.08 | – | 0.13 | % |
| Fe (iron) | 99.2 | – | 99.6 | % |
| Mn (manganese) | 0.3 | – | 0.6 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1010 Annealed Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1010 Annealed Mechanical properties
| Young’s modulus | 205 | – | 215 | GPa |
| Specific stiffness | 26.1 | – | 27.4 | MN.m/kg |
| Yield strength (elastic limit) | 172 | – | 315 | MPa |
| Tensile strength | 310 | – | 430 | MPa |
| Specific strength | 21.9 | – | 40.1 | kN.m/kg |
| Elongation | 29 | – | 45 | % strain |
| Compressive strength | 255 | – | 315 | MPa |
| Flexural modulus | 205 | – | 215 | GPa |
| Flexural strength (modulus of rupture) | 255 | – | 315 | MPa |
| Shear modulus | 79 | – | 84 | GPa |
| Bulk modulus | 158 | – | 175 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 64 | |||
| Hardness – Vickers | 88 | – | 128 | HV |
| Hardness – Rockwell B | 42 | HRB | ||
| Elastic stored energy (springs) | 75.6 | – | 220 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 203 | – | 238 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 160 | – | 302 | MPa |
AISI 1010 Annealed Impact & fracture properties
| Fracture toughness | 43 | – | 69 | MPa.m0.5 |
| Toughness (G) | 9.21 | – | 21.7 | kJ/m2 |
AISI 1010 Annealed Thermal properties
| Melting point | 1490 | – | 1530 | °C |
| Maximum service temperature | 344 | – | 357 | °C |
| Minimum service temperature | -68 | – | -43 | °C |
| Thermal conductivity | 50 | – | 54 | W/m.°C |
| Specific heat capacity | 465 | – | 505 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 13 | µstrain/°C |
| Thermal shock resistance | 66.7 | – | 123 | °C |
| Thermal distortion resistance | 3.96 | – | 4.57 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1010 Annealed Electrical properties
| Electrical resistivity | 13 | – | 16 | µohm.cm |
| Electrical conductivity | 10.8 | – | 13.3 | %IACS |
| Galvanic potential | -0.52 | – | -0.44 | V |
AISI 1010 Annealed Magnetic properties
| Magnetic type | Magnetic | |||
| Remanent induction Br | 0.8 | – | 0.9 | T |
| Saturation induction Bs | 2.15 | T | ||
| Coercive force Hc | 136 | – | 160 | A/m |
| Maximum permeability | 2420 | – | 3800 |
AISI 1010 Annealed Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5110 | – | 5240 | m/s |
| Mechanical loss coefficient (tan delta) | 0.00114 | – | 0.00142 | |
AISI 1010 Annealed Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Excellent |
| Machining speed | 45.7 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Good |
| Carbon equivalency | 0.09 – 0.15 |
AISI 1010 Annealed Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1010 Annealed Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Not susceptible |
AISI 1010 Annealed Standards with similar compositions
| Argentina: IRAM 1010 to IAS, IRAM 1011 to IAS |
| Australia: C1008 to AS 1446, HRC to AS 1594, ICRC to AS 1595, R1008 to AS 1442, R1008 to AS 1443, R1008 to AS 1446, Temper 4 to AS 1585 Part 2, Temper 5 to AS 1585 Part 2, Temper 6 to AS 1585 Part 2 |
| India: 15C4 to IS 11169/1, 15C4 to IS 1570/2/1, 17C 5 to IS 1812, C15 to IS 1570/2/1, CDS-1 to IS 3074, CEW C2 to IS 2039, CEW-1 to IS 3074, Deep Drawing (DD) to IS 12367, Drawing (D) to IS 12367, ERW C2 to IS 2039, ERW-1 to IS 3074, Grade 1 to IS 1673, Grade 2 to IS 1673, Grade 2 to IS 5872, Grade 3 to IS 5872, Grade 4 to IS 7887, Grade 4 to IS 8952, Grade 5 to IS 7887, Grade 5 to IS 8952, IS 11714/2 to IS 11714/2, IS 11714/3 to IS 11714/3, IS 2255 to IS 2255, IS 8057 to IS 8057, YSt 170 Class 1 to IS 1978, YSt 210 to IS 1978 |
| International: CC11X to ISO 4954 |
| Italy: CB10FF to UNI 7356 |
| Japan: SGD 2 to JIS G3108, SWRCH10R to JIS G3507, SWRCH12R to JIS G3507, SWRM 10 to JIS G3505, SWRM 12 to JIS G3505 |
| Mexico: 1010 to NMX-B-301, 1012 to NMX-B-301, B212 to NMX-B-212, Grade A Type S to NMX-B-205, MT1010 to NMX-B-201 |
| Pan America: 1008 to COPANT 330, 1008 to COPANT 331, 1008 to COPANT 333, 1012 to COPANT 333, EP to COPANT 38 |
| Poland: St2N to PN-H-84022, St2N to PN-H-84023/01 |
| Serbia and Montenegro: Z10N |
| South Korea: SGD 2 to KS D 3526, SWRCH10A to KS D 3592, SWRCH10R to KS D 3592, SWRCH12R to KS D 3592, SWRM 10 to KS D 3554, SWRM 12 to KS D 3554 |
| Sweden: 1142-42 to SIS 141142, 1146-32 to SIS 141146, 1146-42 to SIS 141146 |
| Turkey: C12-1/1.0012 to TS 2348, C9-1/1.0010 to TS 2348 |
| UK: 045M10 to BS 970/1, HS12 to BS 1449 Section 1.14, HS15 to BS 1449 Section 1.8 |
| USA: 040 X,Y,Z to SAE J1392, 1010, 1010 to ASTM A29/A29M, 1010 to ASTM A512-96, 1010 to ASTM A513, 1010 to ASTM A519, 1010 to ASTM A568/A568M, 1010 to ASTM A787, 1010 to SAE J403, 1012, 1012 to ASTM A29/A29M, 1012 to ASTM A512-96, 1012 to ASTM A513, 1012 to ASTM A519, 1012 to ASTM A568/A568M, 1012 to MIL-R-8814, 1012 to SAE J403, A179 to ASTM A179/A179M, A2 to ASTM A556/A556M-96, A214 to ASTM A214/A214M, A254 to ASTM A254, A822 to ASTM A822/A822M, C1 to MIL-S-16788A, G10100 to ASTM A510/A510M, G10100 to ASTM A576-90b, G10100 to ASTM A830/A830M, G10120 to ASTM A510/A510M, G10120 to ASTM A576-90b, G10120 to ASTM A830/A830M, Grade A ERW to ASTM A523-96, Grade A Seamless to ASTM A523-96, Grade A to ASTM A1020/A1020M, Grade A to ASTM A178/A178M, Grade B to ASTM A285/A285M, M1010, M1010 to ASTM A29/A29M, M1010 to ASTM A575-96, M1010 to SAE J403, M1012, M1012 to ASTM A29/A29M, M1012 to ASTM A575-96, M1012 to SAE J403, MT1010 to ASTM A512-96, MT1010 to ASTM A513, MT1010 to ASTM A519, MT1010 to ASTM A787, SAE J356 to SAE J356, SAE J524 to SAE J524, SAE J525 to SAE J525, UNS G10100, UNS G10120, UNS K01001, UNS K01200, UNS K01807, UNS K02200, UNS K02201 |
| Tradenames: AIRCO S-10, ASCOMETAL XC10, B&W CARBON STEEL, FORTUNA WO 3, GRANIT 1, KRUPP STE 280 Z, KRUPP STE 280-2 Z, KRUPP STE 280-3 Z, KRUPP UQST 38, KRUPP UST 38, MCKAY 19, NAPAC-35, NAPAC-40, NAPAC-45, NAPAC-50, POMPEY FFC 1, RACO 5, RACO RED LABEL, S-1010, SHARALLOY, SHARALLOY 45, UNA NO. 200, UNA NO. 3200, USS 1110, VERTOMAR 10, VV, WITTEN W 01 E |