PA66 Flame Retarded Grade Material Data Sheet

PA66 Flame Retarded Grade (Polyamide 66) Material Data Sheet

PA66 Flame Retarded Grade Overview

PA66 flame retarded grade is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, Unreinforced, Flame Retarded). This PA66 flame retarded grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 Flame Retarded Grade Designation

Polyamide (Nylon) (Type 66, Unreinforced, Flame Retarded)
TradenamesAddinyl, Adell, Ashlene, Durethan, Frianyl, Hyundai, Kopa, Leona, Nyloy, Plustek, Radiflam, Starflam, Technyl, Vitamide, Wellamid, Zytel

PA66 Flame Retarded Grade Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 Flame Retarded Grade Composition detail

Polymer85–95%
Flame retardant5–15%

PA66 Flame Retarded Grade Physical properties

Density1.15–1.17g/cm3

PA66 Flame Retarded Grade Mechanical properties

Young’s modulus1.63–2.04GPa
Specific stiffness1.4–1.76MN.m/kg
Yield strength (elastic limit)48.7–60.7MPa
Tensile strength40.5–49.5MPa
Specific strength42–52.3kN.m/kg
Elongation19.9–28.7% strain
Elongation at yield12.9–24.5% strain
Compressive modulus1.74–1.93GPa
Compressive strength51.3–56.7MPa
Flexural modulus1.37–1.64GPa
Flexural strength (modulus of rupture)47.7–58.3MPa
Shear modulus0.638–0.671GPa
Shear strength24.3–29.7MPa
Bulk modulus2.93–3.24GPa
Poisson’s ratio0.386–0.401 
Shape factor4.3
Hardness – Vickers16–17HV
Hardness – Rockwell M94–104 
Hardness – Rockwell R94–104 
Hardness – Brinell62–78HB
Hardness – Shore D75–78 
Elastic stored energy (springs)643–1020kJ/m3
Fatigue strength at 10^7 cycles17.1–18.9MPa

PA66 Flame Retarded Grade Impact & fracture properties

Fracture toughness3.46–3.82MPa.m0.5
Toughness (G)6.27–8.38kJ/m2
Impact strength, notched 23 °C3.7–5.9kJ/m2
Impact strength, notched -30 °C1.32–2.88kJ/m2
Impact strength, unnotched 23 °C53.4–96.1kJ/m2

PA66 Flame Retarded Grade Thermal properties

Melting point249–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa210–213°C
Heat deflection temperature 1.8MPa77–93°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.291–0.302W/m.°C
Specific heat capacity1430–1480J/kg.°C
Thermal expansion coefficient79.2–80.8µstrain/°C
Thermal shock resistance319–435°C
Thermal distortion resistance0.00363–0.00379MW/m

PA66 Flame Retarded Grade Electrical properties

Electrical resistivity5.28e19–1.32e21µohm.cm
Electrical conductivity1.31e-19–3.27e-18%IACS
Dielectric constant (relative permittivity)5.23–7.37 
Dissipation factor (dielectric loss tangent)0.0257–0.0677 
Dielectric strength (dielectric breakdown)41.3–70.2MV/m
Comparative tracking index350–600V

PA66 Flame Retarded Grade Magnetic properties

Magnetic typeNon-magnetic

PA66 Flame Retarded Grade Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1180–1330m/s
Mechanical loss coefficient (tan delta)0.0205–0.0227 

PA66 Flame Retarded Grade Absorption & permeability

Water absorption @ 24 hrs0.59–0.96%
Water absorption @ sat6.6–8.7%
Humidity absorption @ sat1.7–2.3%
Water vapor transmission0.865–1.46g.mm/m².day
Permeability (O2)0.339–0.995cm³.mm/m².day.atm

PA66 Flame Retarded Grade Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage1 – 1.6 %
Melt temperature212 – 293 °C
Mold temperature40 – 60 °C
Molding pressure range6.88 – 103 MPa

PA66 Flame Retarded Grade Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySelf-extinguishing