PA6 Cast Heat Resistant Material Data Sheet

PA6 Cast Heat Resistant (Polyamide 6) Material Data Sheet

PA6 Cast Heat Resistant Overview

PA6 cast heat resistant is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Cast, heat stabilized). This PA6 cast heat resistant material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined cast PA6 parts in-house and inspects them before shipment.

PA6 Cast Heat Resistant Designation

Polyamide (Nylon) (Type 6, Cast, heat stabilized)
Tradenames4Mid, Addinyl, Aegis, Akromid, Akulon, Akulon Ultraflow, Alcom, Alphalon, Altech, Amilan, Anjacom, Anjamid, Aquamid, Armamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Capran, Capran Medallion, Chemlon, Clariant, Comco, Compamid, Denyl, Deslon, Dinalon, Distrumid, Domamid, Durethan, Dynacom, Ecotan, Eplamid, Germamid, Glamide, Gravi-Tech, Grilon, Heramid, Hifill, Hylon, Hylonselect, Isocor, Kepamid, Kopa, Lamigamid, LNP Thermocomp, Lumid, Luvocom, Mazmid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nycast, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Nyrim, Orgalloy, Pentamid, Plustek, Polybest, Promyde, Pryme, Quadrant, Radici, Radilon, Scanamid, Schulamid, Selar, Shokamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technamid, Technyl, Technyl Star, Tekamid, Tekumid, Terez, Thermocomp, Thermylon, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Wellamid, Zytel

PA6 Cast Heat Resistant Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 Cast Heat Resistant Composition detail

Polymer100  %

PA6 Cast Heat Resistant Physical properties

Density1.14–1.16g/cm3

PA6 Cast Heat Resistant Mechanical properties

Young’s modulus1.51–1.89GPa
Specific stiffness1.31–1.64MN.m/kg
Yield strength (elastic limit)49–61.1MPa
Tensile strength61.9–75.6MPa
Specific strength42.6–53.1kN.m/kg
Elongation41–59% strain
Elongation at yield5.58–10.6% strain
Compressive modulus1.62–1.79GPa
Compressive strength78.4–86.6MPa
Flexural modulus1.55–1.85GPa
Flexural strength (modulus of rupture)83.9–103MPa
Shear modulus0.609–0.641GPa
Shear strength37.1–45.4MPa
Bulk modulus1.92–2.13GPa
Poisson’s ratio0.34–0.36 
Shape factor4.2
Hardness – Vickers16–17HV
Hardness – Rockwell M119–132 
Hardness – Rockwell R119–132 
Hardness – Shore D83–86 
Elastic stored energy (springs)702–1120kJ/m3
Fatigue strength at 10^7 cycles26.1–28.9MPa

PA6 Cast Heat Resistant Impact & fracture properties

Fracture toughness3.41–3.76MPa.m0.5
Toughness (G)6.57–8.77kJ/m2
Impact strength, notched 23 °C9.4–18.2kJ/m2

PA6 Cast Heat Resistant Thermal properties

Melting point227–238°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa204–221°C
Heat deflection temperature 1.8MPa166–204°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.294–0.306W/m.°C
Specific heat capacity1570–1630J/kg.°C
Thermal expansion coefficient79.4–82.6µstrain/°C
Thermal shock resistance343–467°C
Thermal distortion resistance0.0036–0.00381MW/m

PA6 Cast Heat Resistant Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)5.48–7.72 
Dissipation factor (dielectric loss tangent)0.0825–0.218 
Dielectric strength (dielectric breakdown)14.1–23.9MV/m
Comparative tracking index600  V

PA6 Cast Heat Resistant Magnetic properties

Magnetic typeNon-magnetic

PA6 Cast Heat Resistant Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1140–1280m/s
Mechanical loss coefficient (tan delta)0.0193–0.0213 

PA6 Cast Heat Resistant Absorption & permeability

Water absorption @ 24 hrs0.52–0.84%
Water absorption @ sat5.2–6.8%
Humidity absorption @ sat1.9–2.5%
Water vapor transmission0.958–1.73g.mm/m².day
Permeability (O2)0.622–1.15cm³.mm/m².day.atm

PA6 Cast Heat Resistant Processing properties

Polymer injection moldingUnsuitable
Polymer extrusionUnsuitable
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 1 %

PA6 Cast Heat Resistant Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning