PA6 Cast Grade Material Data Sheet

PA6 Cast Grade (Polyamide 6) Material Data Sheet

PA6 Cast Grade Overview

PA6 cast grade is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Cast). This PA6 cast grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined cast PA6 parts in-house and inspects them before shipment.

PA6 Cast Grade Designation

Polyamide (Nylon) (Type 6, Cast)
Tradenames4Mid, Addinyl, Aegis, Akromid, Akulon, Akulon Ultraflow, Alcom, Alphalon, Altech, Amilan, Anjacom, Anjamid, Aquamid, Armamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Capran, Capran Medallion, Chemlon, Clariant, Comco, Compamid, Denyl, Deslon, Dinalon, Distrumid, Domamid, Durethan, Dynacom, Ecotan, Eplamid, Germamid, Glamide, Gravi-Tech, Grilon, Heramid, Hifill, Hylon, Hylonselect, Isocor, Kepamid, Kopa, Lamigamid, LNP Thermocomp, Lumid, Luvocom, Mazmid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nycast, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Nyrim, Orgalloy, Pentamid, Plustek, Polybest, Promyde, Pryme, Quadrant, Radici, Radilon, Scanamid, Schulamid, Selar, Shokamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technamid, Technyl, Technyl Star, Tekamid, Tekumid, Terez, Thermocomp, Thermylon, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Wellamid, Zytel

PA6 Cast Grade Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 Cast Grade Composition detail

Polymer100  %

PA6 Cast Grade Physical properties

Density1.14–1.16g/cm3

PA6 Cast Grade Mechanical properties

Young’s modulus1.58–1.97GPa
Specific stiffness1.37–1.71MN.m/kg
Yield strength (elastic limit)51.2–63.8MPa
Tensile strength64.7–79.1MPa
Specific strength44.5–55.5kN.m/kg
Elongation61.5–88.5% strain
Elongation at yield5.58–10.6% strain
Compressive modulus1.69–1.86GPa
Compressive strength81.9–90.6MPa
Flexural modulus1.62–1.93GPa
Flexural strength (modulus of rupture)54–66MPa
Shear modulus0.636–0.669GPa
Shear strength38.8–47.4MPa
Bulk modulus2.01–2.22GPa
Poisson’s ratio0.34–0.36 
Shape factor4.2
Hardness – Vickers16–18HV
Hardness – Rockwell M122–135 
Hardness – Rockwell R122–135 
Hardness – Brinell111–139HB
Hardness – Shore D87–93 
Elastic stored energy (springs)735–1170kJ/m3
Fatigue strength at 10^7 cycles27.3–30.2MPa

PA6 Cast Grade Impact & fracture properties

Fracture toughness3.43–3.8MPa.m0.5
Toughness (G)6.39–8.55kJ/m2
Impact strength, notched 23 °C10.2–19.8kJ/m2

PA6 Cast Grade Thermal properties

Melting point227–238°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa204–221°C
Heat deflection temperature 1.8MPa166–204°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.294–0.306W/m.°C
Specific heat capacity1400–1500J/kg.°C
Thermal expansion coefficient88.2–91.8µstrain/°C
Thermal shock resistance309–420°C
Thermal distortion resistance0.00324–0.00343MW/m

PA6 Cast Grade Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)5.48–7.72 
Dissipation factor (dielectric loss tangent)0.077–0.203 
Dielectric strength (dielectric breakdown)13.7–23.3MV/m
Comparative tracking index600  V

PA6 Cast Grade Magnetic properties

Magnetic typeNon-magnetic

PA6 Cast Grade Optical, aesthetic and acoustic properties

Refractive index1.56–1.57 
TransparencyTranslucent
Acoustic velocity1170–1310m/s
Mechanical loss coefficient (tan delta)0.0189–0.0209 

PA6 Cast Grade Absorption & permeability

Water absorption @ 24 hrs0.8–1.3%
Water absorption @ sat5.2–6.8%
Humidity absorption @ sat1.9–2.5%
Water vapor transmission0.958–1.73g.mm/m².day
Permeability (O2)0.622–1.15cm³.mm/m².day.atm

PA6 Cast Grade Processing properties

Polymer injection moldingUnsuitable
Polymer extrusionUnsuitable
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 1 %

PA6 Cast Grade Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning