PA6 Cast Plasticized Material Data Sheet

PA6 Cast Plasticized (Polyamide 6) Material Data Sheet

PA6 Cast Plasticized Overview

PA6 cast plasticized is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Cast, Plasticized). This PA6 cast plasticized material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined cast PA6 parts in-house and inspects them before shipment.

PA6 Cast Plasticized Designation

Polyamide (Nylon) (Type 6, Cast, Plasticized)
TradenamesAshlene, Domamid, Grilon, Radici

PA6 Cast Plasticized Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 Cast Plasticized Composition detail

Polymer77–83%
Plasticizer/oil17–23%

PA6 Cast Plasticized Physical properties

Density1.09–1.12g/cm3

PA6 Cast Plasticized Mechanical properties

Young’s modulus1.2–1.5GPa
Specific stiffness1.09–1.36MN.m/kg
Yield strength (elastic limit)35.6–44.4MPa
Tensile strength45–55MPa
Specific strength32.2–40.2kN.m/kg
Elongation20.5–29.5% strain
Elongation at yield6.77–12.9% strain
Compressive modulus1.28–1.42GPa
Compressive strength57–63MPa
Flexural modulus1.23–1.47GPa
Flexural strength (modulus of rupture)57.4–70.1MPa
Shear modulus0.469–0.493GPa
Shear strength27–33MPa
Bulk modulus2.2–2.44GPa
Poisson’s ratio0.387–0.403 
Shape factor4.3
Hardness – Vickers11–13HV
Hardness – Rockwell M100–110 
Hardness – Rockwell R100–110 
Hardness – Shore D77–80 
Elastic stored energy (springs)467–743kJ/m3
Fatigue strength at 10^7 cycles19–21MPa

PA6 Cast Plasticized Impact & fracture properties

Fracture toughness3.25–3.59MPa.m0.5
Toughness (G)7.52–10.1kJ/m2
Impact strength, notched 23 °C8.06–15.6kJ/m2

PA6 Cast Plasticized Thermal properties

Melting point227–238°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa204–221°C
Heat deflection temperature 1.8MPa166–204°C
Maximum service temperature52–67°C
Minimum service temperature-64–-54°C
Thermal conductivity0.273–0.284W/m.°C
Specific heat capacity1580–1640J/kg.°C
Thermal expansion coefficient79.4–82.6µstrain/°C
Thermal shock resistance313–427°C
Thermal distortion resistance0.00334–0.00353MW/m

PA6 Cast Plasticized Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)5.4–7.61 
Dissipation factor (dielectric loss tangent)0.0825–0.218 
Dielectric strength (dielectric breakdown)10.4–17.6MV/m
Comparative tracking index600  V

PA6 Cast Plasticized Magnetic properties

Magnetic typeNon-magnetic

PA6 Cast Plasticized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1040–1170m/s
Mechanical loss coefficient (tan delta)0.0216–0.0239 

PA6 Cast Plasticized Absorption & permeability

Water absorption @ 24 hrs0.46–0.76%
Water absorption @ sat5.4–7.2%
Humidity absorption @ sat1.7–2.3%
Water vapor transmission0.958–1.73g.mm/m².day
Permeability (O2)0.622–1.15cm³.mm/m².day.atm

PA6 Cast Plasticized Processing properties

Polymer injection moldingUnsuitable
Polymer extrusionUnsuitable
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 1 %

PA6 Cast Plasticized Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning