PA6 Cast Type 612 Blend Material Data Sheet

PA6 Cast Type 612 Blend (Polyamide 6) Material Data Sheet

PA6 Cast Type 612 Blend Overview

PA6 cast type 612 blend is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, Cast, Type 612 Blend). This PA6 cast type 612 blend material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined cast PA6 parts in-house and inspects them before shipment.

PA6 Cast Type 612 Blend Designation

Polyamide (Nylon) (Type 6, Cast, Type 612 Blend)
Tradenames4Mid, Addinyl, Aegis, Akromid, Akulon, Akulon Ultraflow, Alcom, Alphalon, Altech, Amilan, Anjacom, Anjamid, Aquamid, Armamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Capran, Capran Medallion, Chemlon, Clariant, Comco, Compamid, Denyl, Deslon, Dinalon, Distrumid, Domamid, Durethan, Dynacom, Ecotan, Eplamid, Germamid, Glamide, Gravi-Tech, Grilon, Heramid, Hifill, Hylon, Hylonselect, Isocor, Kepamid, Kopa, Lamigamid, LNP Thermocomp, Lumid, Luvocom, Mazmid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nycast, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Nyrim, Orgalloy, Pentamid, Plustek, Polybest, Promyde, Pryme, Quadrant, Radici, Radilon, Scanamid, Schulamid, Selar, Shokamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technamid, Technyl, Technyl Star, Tekamid, Tekumid, Terez, Thermocomp, Thermylon, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Wellamid, Zytel

PA6 Cast Type 612 Blend Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 Cast Type 612 Blend Composition detail

Polymer100  %

PA6 Cast Type 612 Blend Physical properties

Density1.12–1.15g/cm3

PA6 Cast Type 612 Blend Mechanical properties

Young’s modulus1.98–2.47GPa
Specific stiffness1.74–2.18MN.m/kg
Yield strength (elastic limit)43.9–54.7MPa
Tensile strength55.5–67.8MPa
Specific strength38.7–48.2kN.m/kg
Elongation42–60.4% strain
Elongation at yield5.58–10.6% strain
Compressive modulus2.12–2.34GPa
Compressive strength70.3–77.7MPa
Flexural modulus2.03–2.43GPa
Flexural strength (modulus of rupture)73.9–90.3MPa
Shear modulus0.77–0.809GPa
Shear strength33.3–40.7MPa
Bulk modulus3.96–4.38GPa
Poisson’s ratio0.395–0.411 
Shape factor5.02
Hardness – Vickers14–16HV
Hardness – Rockwell M112–124 
Hardness – Rockwell R112–124 
Hardness – Shore D81–84 
Elastic stored energy (springs)431–684kJ/m3
Fatigue strength at 10^7 cycles23.4–25.9MPa

PA6 Cast Type 612 Blend Impact & fracture properties

Fracture toughness3.6–3.97MPa.m0.5
Toughness (G)5.6–7.46kJ/m2
Impact strength, notched 23 °C7.6–14.8kJ/m2

PA6 Cast Type 612 Blend Thermal properties

Melting point204–216°C
Glass temperature40–56°C
Heat deflection temperature 0.45MPa204–216°C
Heat deflection temperature 1.8MPa166–204°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.247–0.257W/m.°C
Specific heat capacity1620–1680J/kg.°C
Thermal expansion coefficient72–81µstrain/°C
Thermal shock resistance247–341°C
Thermal distortion resistance0.0031–0.00351MW/m

PA6 Cast Type 612 Blend Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)5.48–7.72 
Dissipation factor (dielectric loss tangent)0.077–0.203 
Dielectric strength (dielectric breakdown)13.7–23.3MV/m
Comparative tracking index600  V

PA6 Cast Type 612 Blend Magnetic properties

Magnetic typeNon-magnetic

PA6 Cast Type 612 Blend Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1320–1480m/s
Mechanical loss coefficient (tan delta)0.0168–0.0186 

PA6 Cast Type 612 Blend Absorption & permeability

Water absorption @ 24 hrs0.15–0.25%
Water absorption @ sat4.3–5.7%
Humidity absorption @ sat1.9–2.5%
Water vapor transmission0.958–1.73g.mm/m².day
Permeability (O2)0.622–1.15cm³.mm/m².day.atm

PA6 Cast Type 612 Blend Processing properties

Polymer injection moldingUnsuitable
Polymer extrusionUnsuitable
Polymer thermoformingUnsuitable
Linear mold shrinkage0.1 – 1 %

PA6 Cast Type 612 Blend Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning