PEK 20% Glass Fiber Material Data Sheet

PEK 20% Glass Fiber (Polyetherketone) Material Data Sheet

PEK 20% Glass Fiber Overview

PEK 20% glass fiber is a grade of polyetherketone (PEK), designated Polyetherketone (20% Glass Fiber). This PEK 20% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEK parts in-house and inspects them before shipment.

PEK Designation

Polyetherketone (20% Glass Fiber)
TradenamesG-Paek

PEK Typical uses

Bearing cages, gear support bearings, thrust washers, clutch seals, transmission parts, housing for tire pressure sensors, valve spring discs, rollers, guides, gears, reciprocating components.

PEK 20% Glass Fiber Composition detail

Polymer80  %
Glass (fiber)20  %

PEK Physical properties

Density1.44–1.46g/cm3

PEK 20% Glass Fiber Mechanical properties

Young’s modulus8.88–9.33GPa
Specific stiffness6.12–6.44MN.m/kg
Yield strength (elastic limit)130–143MPa
Tensile strength162–179MPa
Specific strength89.3–98.8kN.m/kg
Elongation3.07–3.55% strain
Compressive modulus8.88–9.33GPa
Compressive strength156–172MPa
Flexural modulus8.88–9.33GPa
Flexural strength (modulus of rupture)229–252MPa
Shear modulus3.27–3.44GPa
Bulk modulus10.4–10.9GPa
Poisson’s ratio0.35–0.365 
Shape factor6.3
Hardness – Vickers39–43HV
Hardness – Rockwell M95–105 
Hardness – Rockwell R119–131 
Elastic stored energy (springs)922–1130kJ/m3
Fatigue strength at 10^7 cycles59.8–77.8MPa

PEK Impact & fracture properties

Fracture toughness4.01–7.85MPa.m0.5
Toughness (G)1.92–6.22kJ/m2
Impact strength, notched 23 °C7.3–8.1kJ/m2

PEK 20% Glass Fiber Thermal properties

Melting point368–394°C
Glass temperature182–200°C
Heat deflection temperature 0.45MPa282–339°C
Heat deflection temperature 1.8MPa225–276°C
Vicat softening point282–339°C
Maximum service temperature215–234°C
Minimum service temperature-47–-27°C
Thermal conductivity0.454–0.472W/m.°C
Specific heat capacity1340–1400J/kg.°C
Thermal expansion coefficient44.1–45.9µstrain/°C
Thermal shock resistance314–353°C
Thermal distortion resistance0.01–0.0106MW/m

PEK Electrical properties

Electrical resistivity3300000000000000000000–30000000000000000000000µohm.cm
Electrical conductivity5.75e-21–5.22e-20%IACS
Dielectric constant (relative permittivity)3.14–3.46 
Dissipation factor (dielectric loss tangent)0.00398–0.00477 
Dielectric strength (dielectric breakdown)13–15MV/m
Comparative tracking index175–225V

PEK Magnetic properties

Magnetic typeNon-magnetic

PEK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2470–2540m/s
Mechanical loss coefficient (tan delta)0.00838–0.00867 

PEK Absorption & permeability

Water absorption @ 24 hrs0.06–0.08%

PEK Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingUnsuitable
Linear mold shrinkage0.818 – 0.99 %
Melt temperature344 – 430 °C
Molding pressure range68.8 – 138 MPa

PEK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySelf-extinguishing