Home » High Conductivity Copper » C18200 H.C. Copper, Solution Treated & Aged Material Data Sheet
C18200 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Aged)
C18200 Solution Treated Aged Copper Overview
C18200 solution treated aged copper is a wrought high conductivity copper (UNS C18200, EN CW105C), known as h.c. copper. Condition: Solution heat-treated & precipitation hardened. This C18200 solution treated aged copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C18200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C18200 copper parts in-house and inspects them before shipment.
C18200 Designation
Copper Alloy: hc-CuCr1(wp) (UNS C18200) Condition Solution heat-treated & precipitation hardened UNS number C18200 EN name CW105C ISO name CuCr1 JIS (Japanese) name C1820
C18200 Typical uses
Cable connectors, switchgear & circuit breakers, commutator bars & end-rings for electrical motors, electronic devices, contact wheels.
C18200 Solution Treated Aged Copper Composition detail
Cr (chromium) 0.6 – 1.2 % Cu (copper) 98.6 – 99.4 % Fe (iron) 0 – 0.1 % Pb (lead) 0 – 0.05 % Si (silicon) 0 – 0.1 %
C18200 Physical properties
C18200 Solution Treated Aged Copper Mechanical properties
Young’s modulus 140 – 150 GPa Specific stiffness 15.7 – 16.8 MN.m/kg Yield strength (elastic limit) 290 – 310 MPa Tensile strength 405 – 420 MPa Specific strength 32.4 – 34.7 kN.m/kg Elongation 14 – 16 % strain Compressive strength 290 – 310 MPa Flexural modulus 140 – 150 GPa Flexural strength (modulus of rupture) 290 – 310 MPa Shear modulus 52 – 55 GPa Bulk modulus 151 – 162 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 27 Hardness – Vickers 130 – 138 HV Elastic stored energy (springs) 288 – 334 kJ/m3 Fatigue strength at 10^7 cycles 170 – 200 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 169 – 202 MPa
C18200 Impact & fracture properties
Fracture toughness 41.3 – 43.2 MPa.m0.5 Toughness (G) 11.6 – 13 kJ/m2
C18200 Solution Treated Aged Copper Thermal properties
Melting point 1070 – 1080 °C Maximum service temperature 77 – 87 °C Minimum service temperature -273 °C Thermal conductivity 300 – 340 W/m.°C Specific heat capacity 372 – 380 J/kg.°C Thermal expansion coefficient 16.9 – 17.1 µstrain/°C Thermal shock resistance 116 – 128 °C Thermal distortion resistance 17.6 – 20 MW/m Latent heat of fusion 200 – 208 kJ/kg
C18200 Electrical properties
Electrical resistivity 2 – 2.29 µohm.cm Electrical conductivity 75.3 – 86.2 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.19 – -0.11 V
C18200 Magnetic properties
Magnetic type Non-magnetic
C18200 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3960 – 4100 m/s Mechanical loss coefficient (tan delta) 4.2e-5 – 4.8e-5
C18200 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Acceptable Metal press forming Excellent Metal deep drawing Limited use Machining speed 33.5 m/min Weldability Notes: Preheating and post weld heat treatment are not required Good
C18200 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C18200 Solution Treated Aged Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C18200 Notes
C18200 Solution Treated Aged Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C18200 Standards with similar compositions
Europe: CW105C to CEN EN 12163, CW105C to CEN EN 12165, CW105C to CEN EN 12167, CW105C to CEN EN 12420Germany: 2.1291 to DIN, CuCrZr to DINInternational: CuCr1 to ISO 1637, CuCr1 to ISO 1640, CuCr1 to ISO R1336Japan: CuCr1 to JIS Z3234USA: 99Cu-1Cr to ASTM F9, C18200, UNS C18200Tradenames: AMCROM, AMPCOLOY 98, AMPCO-TRODE 182, ANACONDA 182, BOLTOMET 814, BOLTOMET 818, BRUSH CHROMIUM COPPER, CERRO CCS, CHROMIUM COPPER-182, CHROMIUM-COPPER 999, CUPROCHROME, ERM CCS, ERM CCS (M3), HIDUREL 6, MITSUBISHI MKC, MUELLER 1820
Modulus Metal Services
Manufacturing & Quality Services in Turkey