C18200 H.C. Copper, Solution Treated & Work Hardened Material Data Sheet

C18200 H.C. Copper Material Data Sheet (Wrought, Solution Treated & Work Hardened)

C18200 Solution Treated Cold Worked Copper Overview

C18200 solution treated cold worked copper is a wrought high conductivity copper (UNS C18200, EN CW105C), known as h.c. copper. Condition: Solution heat-treated & work hardened. This C18200 solution treated cold worked copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C18200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C18200 copper parts in-house and inspects them before shipment.

C18200 Designation

Copper Alloy: hc-CuCr1(wh); A2/1 (UNS C18200)
ConditionSolution heat-treated & work hardened
UNS numberC18200
EN nameCW105C
ISO nameCuCr1
JIS (Japanese) nameC1820

C18200 Typical uses

Cable connectors, switchgear & circuit breakers, commutator bars & end-rings for electrical motors, electronic devices, contact wheels.

C18200 Solution Treated Cold Worked Copper Composition detail

Cr (chromium)0.6–1.2%
Cu (copper)98.6–99.4%
Fe (iron)0–0.1%
Pb (lead)0–0.05%
Si (silicon)0–0.1%

C18200 Physical properties

Density8.94–8.95g/cm3

C18200 Solution Treated Cold Worked Copper Mechanical properties

Young’s modulus110–115GPa
Specific stiffness12.3–12.9MN.m/kg
Yield strength (elastic limit)180–290MPa
Tensile strength350–510MPa
Specific strength20.1–32.4kN.m/kg
Elongation4–7% strain
Compressive strength180–290MPa
Flexural modulus110–115GPa
Flexural strength (modulus of rupture)180–290MPa
Shear modulus41–42GPa
Bulk modulus119–124GPa
Poisson’s ratio0.34–0.35 
Shape factor27
Hardness – Vickers115–130HV
Elastic stored energy (springs)151–357kJ/m3
Fatigue strength at 10^7 cycles160–180MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
120–241MPa

C18200 Impact & fracture properties

Fracture toughness43.2–57.6MPa.m0.5
Toughness (G)16.9–29kJ/m2

C18200 Solution Treated Cold Worked Copper Thermal properties

Melting point1070–1080°C
Maximum service temperature300–350°C
Minimum service temperature-273  °C
Thermal conductivity160–170W/m.°C
Specific heat capacity372–380J/kg.°C
Thermal expansion coefficient16.9–17.1µstrain/°C
Thermal shock resistance94.1–152°C
Thermal distortion resistance9.41–10MW/m
Latent heat of fusion200–208kJ/kg

C18200 Electrical properties

Electrical resistivity4.9–5.13µohm.cm
Electrical conductivity33.6–35.2%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.19–-0.11V

C18200 Magnetic properties

Magnetic typeNon-magnetic

C18200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3510–3590m/s
Mechanical loss coefficient (tan delta)4.8e-5–1.23e-4 

C18200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed33.5 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C18200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C18200 Solution Treated Cold Worked Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C18200 Notes

C18200 Solution Treated Cold Worked Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C18200 Standards with similar compositions

Europe: CW105C to CEN EN 12163, CW105C to CEN EN 12165, CW105C to CEN EN 12167, CW105C to CEN EN 12420
Germany: 2.1291 to DIN, CuCrZr to DIN
International: CuCr1 to ISO 1637, CuCr1 to ISO 1640, CuCr1 to ISO R1336
Japan: CuCr1 to JIS Z3234
USA: 99Cu-1Cr to ASTM F9, C18200, UNS C18200
Tradenames: AMCROM, AMPCOLOY 98, AMPCO-TRODE 182, ANACONDA 182, BOLTOMET 814, BOLTOMET 818, BRUSH CHROMIUM COPPER, CERRO CCS, CHROMIUM COPPER-182, CHROMIUM-COPPER 999, CUPROCHROME, ERM CCS, ERM CCS (M3), HIDUREL 6, MITSUBISHI MKC, MUELLER 1820