C14500 H.C. Copper Material Data Sheet (Wrought, Hard)
C14500 Hard Copper Overview
C14500 hard copper is a wrought high conductivity copper (UNS C14500), known as h.c. copper. Condition: Hard. This C14500 hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14500 copper parts in-house and inspects them before shipment.
C14500 Designation
Wrought Copper Alloy: hc-CuTe(h); C109
Condition
Hard
UNS number
C14500
C14500 Hard Copper Composition detail
Cu (copper)
99.3
–
99.6
%
P (phosphorus)
0.004
–
0.012
%
Te (tellurium)
0.4
–
0.7
%
C14500 Physical properties
Density
8.94
–
8.95
g/cm3
C14500 Hard Copper Mechanical properties
Young’s modulus
125
–
132
GPa
Specific stiffness
14
–
14.8
MN.m/kg
Yield strength (elastic limit)
250
–
320
MPa
Tensile strength
280
–
350
MPa
Specific strength
28
–
35.8
kN.m/kg
Elongation
4
–
15
% strain
Compressive strength
250
–
320
MPa
Flexural modulus
125
–
132
GPa
Flexural strength (modulus of rupture)
250
–
320
MPa
Shear modulus
47.4
–
50
GPa
Bulk modulus
135
–
143
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
26
Hardness – Vickers
90
–
110
HV
Elastic stored energy (springs)
246
–
394
kJ/m3
Fatigue strength at 10^7 cycles
110
–
120
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
91.8
–
144
MPa
C14500 Impact & fracture properties
Fracture toughness
40.4
–
47.5
MPa.m0.5
Toughness (G)
12.8
–
17.5
kJ/m2
C14500 Hard Copper Thermal properties
Melting point
977
–
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
365
–
376
W/m.°C
Specific heat capacity
375
–
385
J/kg.°C
Thermal expansion coefficient
16.8
–
16.9
µstrain/°C
Thermal shock resistance
115
–
148
°C
Thermal distortion resistance
21.7
–
22.3
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C14500 Electrical properties
Electrical resistivity
1.78
–
1.86
µohm.cm
Electrical conductivity
92.7
–
96.9
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C14500 Magnetic properties
Magnetic type
Non-magnetic
C14500 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3740
–
3840
m/s
Mechanical loss coefficient (tan delta)
3.9e-5
–
6.4e-5
C14500 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
29 m/min
Weldability
Unsuitable
C14500 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C14500 Hard Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C14500 Notes
C14500 Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C14500 Standards with similar compositions
Australia: 145 to AS 1567
Europe: CW118C to CEN EN 12164, CW118C to CEN EN 12166, CW118C to CEN EN 12168
International: CuTe to ISO 1637, CuTe to ISO R1336, CuTe(P) to ISO 1637, CuTe(P) to ISO R1336
UK: C109 to BS 2874
USA: C14500, C14500 to ASTM B124M, C14500 to ASTM B283, C14500 to ASTM B301/B301M, C14500 to SAE J463, C14510, C14510 to ASTM B301/B301M, C14520, C14520 to ASTM B301/B301M, UNS C14500, UNS C14510, UNS C14520