C14500 H.C. Copper Material Data Sheet (Wrought, Soft)
C14500 Soft Copper Overview
C14500 soft copper is a wrought high conductivity copper (UNS C14500), known as h.c. copper. Condition: Soft. This C14500 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C14500 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C14500 copper parts in-house and inspects them before shipment.
C14500 Designation
Wrought Copper Alloy: hc-CuTe(s); C109
Condition
Soft
UNS number
C14500
C14500 Soft Copper Composition detail
Cu (copper)
99.3
–
99.6
%
P (phosphorus)
0.004
–
0.012
%
Te (tellurium)
0.4
–
0.7
%
C14500 Physical properties
Density
8.94
–
8.95
g/cm3
C14500 Soft Copper Mechanical properties
Young’s modulus
122
–
128
GPa
Specific stiffness
13.6
–
14.3
MN.m/kg
Yield strength (elastic limit)
55
–
65
MPa
Tensile strength
220
–
240
MPa
Specific strength
6.15
–
7.27
kN.m/kg
Elongation
38
–
42
% strain
Compressive strength
55
–
65
MPa
Flexural modulus
122
–
128
GPa
Flexural strength (modulus of rupture)
55
–
65
MPa
Shear modulus
44
–
46
GPa
Bulk modulus
132
–
138
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
53
–
56
HV
Elastic stored energy (springs)
12.2
–
16.8
kJ/m3
Fatigue strength at 10^7 cycles
90
–
110
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
87.3
–
113
MPa
C14500 Impact & fracture properties
Fracture toughness
88.4
–
92.7
MPa.m0.5
Toughness (G)
62.2
–
69.1
kJ/m2
C14500 Soft Copper Thermal properties
Melting point
977
–
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
365
–
376
W/m.°C
Specific heat capacity
375
–
385
J/kg.°C
Thermal expansion coefficient
16.8
–
16.9
µstrain/°C
Thermal shock resistance
26
–
31
°C
Thermal distortion resistance
21.7
–
22.3
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C14500 Electrical properties
Electrical resistivity
1.74
–
1.82
µohm.cm
Electrical conductivity
94.7
–
99.1
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C14500 Magnetic properties
Magnetic type
Non-magnetic
C14500 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3690
–
3780
m/s
Mechanical loss coefficient (tan delta)
9.47e-4
–
0.00132
C14500 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
29 m/min
Weldability
Unsuitable
C14500 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C14500 Soft Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C14500 Notes
C14500 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C14500 Standards with similar compositions
Australia: 145 to AS 1567
Europe: CW118C to CEN EN 12164, CW118C to CEN EN 12166, CW118C to CEN EN 12168
International: CuTe to ISO 1637, CuTe to ISO R1336, CuTe(P) to ISO 1637, CuTe(P) to ISO R1336
UK: C109 to BS 2874
USA: C14500, C14500 to ASTM B124M, C14500 to ASTM B283, C14500 to ASTM B301/B301M, C14500 to SAE J463, C14510, C14510 to ASTM B301/B301M, C14520, C14520 to ASTM B301/B301M, UNS C14500, UNS C14510, UNS C14520