C10200 Oxygen-Free H.C. Copper, Half Hard Material Data Sheet

C10200 Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Half Hard)

C10200 Half Hard Copper Overview

C10200 half hard copper is a wrought high conductivity copper (UNS C10200, EN CW008A), known as oxygen-free h.c. copper. Condition: Half hard. This C10200 half hard copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10200 copper parts in-house and inspects them before shipment.

C10200 Designation

Wrought Copper Alloy: hc-Cu-OF(1/2h) (UNS C10200)
ConditionHalf hard
UNS numberC10200
EN nameCW008A
ISO nameCu-OF
GB (Chinese) nameTU2
JIS (Japanese) nameC1020

C10200 Typical uses

Conductors, motor & generator windings, waveguides, flexible cable.

C10200 Half Hard Copper Composition detail

Cu (copper)100  %

C10200 Physical properties

Density8.94–8.95g/cm3

C10200 Half Hard Copper Mechanical properties

Young’s modulus125–128GPa
Specific stiffness14–14.3MN.m/kg
Yield strength (elastic limit)150–200MPa
Tensile strength220–310MPa
Specific strength16.8–22.4kN.m/kg
Elongation30–40% strain
Compressive strength150–200MPa
Flexural modulus125–128GPa
Flexural strength (modulus of rupture)150–200MPa
Shear modulus45–48GPa
Bulk modulus135–138GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers55–80HV
Elastic stored energy (springs)90.5–155kJ/m3
Fatigue strength at 10^7 cycles100–115MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
77.4–149MPa

C10200 Impact & fracture properties

Fracture toughness54.3–63.3MPa.m0.5
Toughness (G)23.4–31.5kJ/m2

C10200 Half Hard Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity390–398W/m.°C
Specific heat capacity383–388J/kg.°C
Thermal expansion coefficient16.8–17.3µstrain/°C
Thermal shock resistance69.5–92.8°C
Thermal distortion resistance22.7–23.5MW/m
Latent heat of fusion200–208kJ/kg

C10200 Electrical properties

Electrical resistivity1.7–1.74µohm.cm
Electrical conductivity99.1–101%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C10200 Magnetic properties

Magnetic typeNon-magnetic

C10200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3740–3780m/s
Mechanical loss coefficient (tan delta)1e-4–1.78e-4 

C10200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C10200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C10200 Half Hard Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C10200 Notes

C10200 Half Hard Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C10200 Standards with similar compositions

Canada: Cu-DLP(120) to CSA
Czech Republic: Cu99.75 to CSN 423004, Cu99.85 to CSN 423003
Germany: 2.009 to DIN, Ms58 to DIN, SF-Cu to DIN
Mexico: DLP to DGN W-23
USA: BVCu-1x to AWS A5.8, C10100 to ASTM B111M, C10100 to ASTM B359M, C10100 to ASTM B640, C15150, C71630, ECu to AWS A5.6, OFXLP to ASTM B12, OFXLP to ASTM B133, UNS C14440, UNS C15150
Tradenames: 1200, AMAX MZ COPPER, B-D CU, CADMIUM COPPER, 0.1% CADMIUM, CDA COPPER 109, IMI 149, IMI 161 (BOROFIL), THIN FIN