C10200 Oxygen-Free H.C. Copper, Soft Material Data Sheet

C10200 Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Soft)

C10200 Soft Copper Overview

C10200 soft copper is a wrought high conductivity copper (UNS C10200, EN CW008A), known as oxygen-free h.c. copper. Condition: Soft. This C10200 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10200 copper parts in-house and inspects them before shipment.

C10200 Designation

Wrought Copper Alloy: hc-Cu-OF(s); C103 (UNS C10200)
ConditionSoft
UNS numberC10200
EN nameCW008A
ISO nameCu-OF
GB (Chinese) nameTU2
JIS (Japanese) nameC1020

C10200 Typical uses

Conductors, motor & generator windings, waveguides, flexible cable.

C10200 Soft Copper Composition detail

Cu (copper)100  %

C10200 Physical properties

Density8.94–8.95g/cm3

C10200 Soft Copper Mechanical properties

Young’s modulus120–125GPa
Specific stiffness13.4–14MN.m/kg
Yield strength (elastic limit)45–55MPa
Tensile strength210–230MPa
Specific strength5.03–6.15kN.m/kg
Elongation46–50% strain
Compressive strength45–55MPa
Flexural modulus120–125GPa
Flexural strength (modulus of rupture)45–55MPa
Shear modulus44–46GPa
Bulk modulus130–135GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers48–53HV
Elastic stored energy (springs)8.34–12.2kJ/m3
Fatigue strength at 10^7 cycles70–90MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
68.2–92.4MPa

C10200 Impact & fracture properties

Fracture toughness92.7–97.4MPa.m0.5
Toughness (G)69.9–77.7kJ/m2

C10200 Soft Copper Thermal properties

Melting point1080  °C
Maximum service temperature77–87°C
Minimum service temperature-273  °C
Thermal conductivity390–398W/m.°C
Specific heat capacity383–388J/kg.°C
Thermal expansion coefficient16.8–17.3µstrain/°C
Thermal shock resistance21.5–26.4°C
Thermal distortion resistance22.7–23.5MW/m
Latent heat of fusion200–208kJ/kg

C10200 Electrical properties

Electrical resistivity1.7–1.74µohm.cm
Electrical conductivity99.1–101%IACS
Temperature dependence of resistivity5.2–5.4/°C
Galvanic potential-0.2–-0.12V

C10200 Magnetic properties

Magnetic typeNon-magnetic

C10200 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3660–3740m/s
Mechanical loss coefficient (tan delta)0.00132–0.00198 

C10200 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed29 m/min
Weldability
Notes: Preheating and post weld heat treatment are not required
Good

C10200 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

C10200 Soft Copper Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible

C10200 Notes

C10200 Soft Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C10200 Standards with similar compositions

Canada: Cu-DLP(120) to CSA
Czech Republic: Cu99.75 to CSN 423004, Cu99.85 to CSN 423003
Germany: 2.009 to DIN, Ms58 to DIN, SF-Cu to DIN
Mexico: DLP to DGN W-23
USA: BVCu-1x to AWS A5.8, C10100 to ASTM B111M, C10100 to ASTM B359M, C10100 to ASTM B640, C15150, C71630, ECu to AWS A5.6, OFXLP to ASTM B12, OFXLP to ASTM B133, UNS C14440, UNS C15150
Tradenames: 1200, AMAX MZ COPPER, B-D CU, CADMIUM COPPER, 0.1% CADMIUM, CDA COPPER 109, IMI 149, IMI 161 (BOROFIL), THIN FIN