C10200 Oxygen-Free H.C. Copper, Hot Rolled Material Data Sheet
C10200 Oxygen-Free H.C. Copper Material Data Sheet (Wrought, Hot Rolled)
C10200 Hot Rolled Copper Overview
C10200 hot rolled copper is a wrought high conductivity copper (UNS C10200, EN CW008A), known as oxygen-free h.c. copper. Condition: Hot rolled. This C10200 hot rolled copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C10200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C10200 copper parts in-house and inspects them before shipment.
C10200 Designation
Wrought Copper Alloy: hc-Cu-OF(hr) (UNS C10200)
Condition
Hot rolled
UNS number
C10200
EN name
CW008A
ISO name
Cu-OF
GB (Chinese) name
TU2
JIS (Japanese) name
C1020
C10200 Typical uses
Conductors, motor & generator windings, waveguides, flexible cable.
C10200 Hot Rolled Copper Composition detail
Cu (copper)
100
%
C10200 Physical properties
Density
8.94
–
8.95
g/cm3
C10200 Hot Rolled Copper Mechanical properties
Young’s modulus
124
–
128
GPa
Specific stiffness
13.9
–
14.3
MN.m/kg
Yield strength (elastic limit)
75
–
85
MPa
Tensile strength
220
–
240
MPa
Specific strength
8.39
–
9.51
kN.m/kg
Elongation
37
–
42
% strain
Compressive strength
75
–
85
MPa
Flexural modulus
124
–
128
GPa
Flexural strength (modulus of rupture)
75
–
85
MPa
Shear modulus
45
–
48
GPa
Bulk modulus
134
–
138
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
30
Hardness – Vickers
58
–
64
HV
Elastic stored energy (springs)
22.4
–
28.6
kJ/m3
Fatigue strength at 10^7 cycles
75
–
95
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
73
–
97.6
MPa
C10200 Impact & fracture properties
Fracture toughness
80.9
–
84.4
MPa.m0.5
Toughness (G)
51.8
–
56.7
kJ/m2
C10200 Hot Rolled Copper Thermal properties
Melting point
1080
°C
Maximum service temperature
77
–
87
°C
Minimum service temperature
-273
°C
Thermal conductivity
390
–
398
W/m.°C
Specific heat capacity
383
–
388
J/kg.°C
Thermal expansion coefficient
16.8
–
17.3
µstrain/°C
Thermal shock resistance
34.8
–
39.7
°C
Thermal distortion resistance
22.7
–
23.5
MW/m
Latent heat of fusion
200
–
208
kJ/kg
C10200 Electrical properties
Electrical resistivity
1.7
–
1.74
µohm.cm
Electrical conductivity
99.1
–
101
%IACS
Temperature dependence of resistivity
5.2
–
5.4
/°C
Galvanic potential
-0.2
–
-0.12
V
C10200 Magnetic properties
Magnetic type
Non-magnetic
C10200 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3720
–
3780
m/s
Mechanical loss coefficient (tan delta)
5.54e-4
–
7.11e-4
C10200 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
29 m/min
Weldability Notes: Preheating and post weld heat treatment are not required
Good
C10200 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
C10200 Hot Rolled Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Not susceptible
C10200 Notes
C10200 Hot Rolled Copper Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C10200 Standards with similar compositions
Canada: Cu-DLP(120) to CSA
Czech Republic: Cu99.75 to CSN 423004, Cu99.85 to CSN 423003
Germany: 2.009 to DIN, Ms58 to DIN, SF-Cu to DIN
Mexico: DLP to DGN W-23
USA: BVCu-1x to AWS A5.8, C10100 to ASTM B111M, C10100 to ASTM B359M, C10100 to ASTM B640, C15150, C71630, ECu to AWS A5.6, OFXLP to ASTM B12, OFXLP to ASTM B133, UNS C14440, UNS C15150