Home » Gunmetal Alloys » 87-7-3-3 (C92410) Leaded Gunmetal, Cast Material Data Sheet
87-7-3-3 (C92410) Leaded Gunmetal, Cast Material Data Sheet
87-7-3-3 (C92410) Leaded Gunmetal Material Data Sheet (Cast)
C92410 Cast Gunmetal Overview
C92410 cast gunmetal is a cast gunmetal (UNS C92410), known as leaded gunmetal. Condition: Cast. This C92410 cast gunmetal material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C92410 gunmetal castings from Turkey (Türkiye)? Modulus Metal supplies C92410 gunmetal castings with in-house CNC machining and inspects them before shipment.
C92410 Designation
87-7-3-3
UNS number
C92410
ISO name
CuSn7Zn2Pb3
C92410 Typical uses
Pumps, valves, housings to resist corrosion, low-stressed bushings.
C92410 Cast Gunmetal Composition detail
Al (aluminum)
0
–
0.005
%
Bi (bismuth)
0
–
0.05
%
Cu (copper)
84.7
–
90
%
Fe (iron)
0
–
0.2
%
Mn (manganese)
0
–
0.05
%
Ni (nickel)
0
–
0.2
%
Pb (lead)
2.5
–
3.5
%
Sb (antimony)
0
–
0.25
%
Si (silicon)
0
–
0.005
%
Sn (tin)
6
–
8
%
Zn (zinc)
1.5
–
3
%
C92410 Physical properties
Density
8.75
–
8.85
g/cm3
C92410 Cast Gunmetal Mechanical properties
Young’s modulus
79
–
82
GPa
Specific stiffness
8.97
–
9.33
MN.m/kg
Yield strength (elastic limit)
130
–
160
MPa
Tensile strength
250
–
340
MPa
Specific strength
14.8
–
18.2
kN.m/kg
Elongation
5
–
15
% strain
Compressive strength
130
–
160
MPa
Flexural modulus
79
–
82
GPa
Flexural strength (modulus of rupture)
130
–
160
MPa
Shear modulus
29.2
–
30.3
GPa
Bulk modulus
85.3
–
88.6
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
80
–
95
HV
Elastic stored energy (springs)
106
–
158
kJ/m3
Fatigue strength at 10^7 cycles
130
–
159
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
106
–
195
MPa
C92410 Impact & fracture properties
Fracture toughness
61.3
–
67.9
MPa.m0.5
Toughness (G)
46.7
–
57.2
kJ/m2
C92410 Cast Gunmetal Thermal properties
Melting point
917
–
1040
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-63
–
-48
°C
Thermal conductivity
60
–
65
W/m.°C
Specific heat capacity
383
–
384
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
89.4
–
111
°C
Thermal distortion resistance
3.31
–
3.64
MW/m
Latent heat of fusion
220
–
240
kJ/kg
C92410 Electrical properties
Electrical resistivity
13.2
–
17.4
µohm.cm
Electrical conductivity
9.91
–
13.1
%IACS
Galvanic potential
-0.24
–
-0.16
V
C92410 Magnetic properties
Magnetic type
Non-magnetic
C92410 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2990
–
3050
m/s
Mechanical loss coefficient (tan delta)
1.56e-4
–
2.37e-4
C92410 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
64 m/min
Weldability
Unsuitable
C92410 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
C92410 Cast Gunmetal Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible
C92410 Notes
C92410 Cast Gunmetal Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C92410 Standards with similar compositions
Australia: C92410A to AS 2738
Europe: CB492K to CEN EN 1982, CC492K to CEN EN 1982