ASTM CB-7Cu Cast Aged at 550°C Stainless Steel Material Data Sheet

ASTM CB-7Cu Aged at 550°C Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

ASTM CB-7Cu Aged at 550°C Overview

CB-7Cu aged at 550°C is a martensitic precipitation hardening stainless steel (UNS J92180) in the cast form. Condition: Solution annealed; precipitation (age) hardened at 550°C; air cooled. This CB-7Cu aged at 550°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for ASTM CB-7Cu castings from Turkey (Türkiye)? Modulus Metal supplies ASTM CB-7Cu castings with in-house CNC machining and inspects them before shipment.

ASTM CB-7Cu Designation

ASTM CB-7Cu
ConditionSolution annealed; precipitation (age) hardened at 550°C; air cooled
UNS numberJ92180
US nameASTM CB-7Cu

ASTM CB-7Cu Typical uses

Aerospace, chemical processing, food processing, gas turbine, marine, petrochemical industry, pulp and paper industries

ASTM CB-7Cu Aged at 550°C Composition detail

C (carbon)0–0.07%
Cr (chromium)15.5–17.7%
Cu (copper)2.5–3.2%
Fe (iron)72.3–78.2%
Mn (manganese)0–0.7%
N (nitrogen)0–0.05%
Nb (niobium)0.15–0.35%
Ni (nickel)3.6–4.6%
P (phosphorus)0–0.035%
S (sulfur)0–0.03%
Si (silicon)0–1%

ASTM CB-7Cu Physical properties

Density7.7–7.8g/cm3

ASTM CB-7Cu Aged at 550°C Mechanical properties

Young’s modulus190–200GPa
Specific stiffness24.5–25.8MN.m/kg
Yield strength (elastic limit)1020–1150MPa
Tensile strength1040–1250MPa
Specific strength132–148kN.m/kg
Elongation11–17% strain
Compressive strength1030–1150MPa
Flexural modulus190–200GPa
Flexural strength (modulus of rupture)1040–1150MPa
Shear modulus73–79GPa
Bulk modulus140–156GPa
Poisson’s ratio0.275–0.285 
Shape factor21
Hardness – Vickers340–360HV
Hardness – Rockwell C33–38HRC
Hardness – Brinell314–349HB
Elastic stored energy (springs)2670–3360kJ/m3
Fatigue strength at 10^7 cycles434–501MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
384–566MPa

ASTM CB-7Cu Impact & fracture properties

Fracture toughness27–40MPa.m0.5
Toughness (G)3.86–7.95kJ/m2

ASTM CB-7Cu Aged at 550°C Thermal properties

Melting point1490–1530°C
Maximum service temperature700–750°C
Minimum service temperature-73–-43°C
Thermal conductivity15–19W/m.°C
Specific heat capacity450–470J/kg.°C
Thermal expansion coefficient9.5–12.5µstrain/°C
Thermal shock resistance438–591°C
Thermal distortion resistance1.3–1.85MW/m
Latent heat of fusion260–285kJ/kg

ASTM CB-7Cu Electrical properties

Electrical resistivity72–82µohm.cm
Electrical conductivity2.1–2.39%IACS
Galvanic potential-0.19–-0.11V

ASTM CB-7Cu Magnetic properties

Magnetic typeMagnetic

ASTM CB-7Cu Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4950–5080m/s
Mechanical loss coefficient (tan delta)3.5e-4–4.1e-4 

ASTM CB-7Cu Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed12.8 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency0.66 – 0.9

ASTM CB-7Cu Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

ASTM CB-7Cu Aged at 550°C Corrosion resistance

Pitting resistance equivalent number (PREN)15.5 – 18.5
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Not susceptible

ASTM CB-7Cu Notes

ASTM CB-7Cu Aged at 550°C Warning
Castings intended to be welded should have Cu content <3%, to avoid underbead cracking.
ASTM CB-7Cu Aged at 550°C Other notes
Lime-coated electrodes of similar composition should be used for welding by shielded metal-arc process.

ASTM CB-7Cu Standards with similar compositions

India: Grade 1 to IS 11758
Japan: SCS24 to JIS G5121
South Korea: SSC 24 to KS D 4103
USA: CB7Cu-1 to ASTM A747/A747M
Tradenames: HENRICOT HR.34, LEBANON 17-4, SOLEIL C3M, ZCR 174