ASTM CB-7Cu Cast Aged at 480°C Stainless Steel Material Data Sheet
ASTM CB-7Cu Aged at 480°C Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
ASTM CB-7Cu Aged at 480°C Overview
CB-7Cu aged at 480°C is a martensitic precipitation hardening stainless steel (UNS J92180) in the cast form. Condition: Solution annealed; precipitation (age) hardened at 480°C; air cooled. This CB-7Cu aged at 480°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for ASTM CB-7Cu castings from Turkey (Türkiye)? Modulus Metal supplies ASTM CB-7Cu castings with in-house CNC machining and inspects them before shipment.
ASTM CB-7Cu Designation
ASTM CB-7Cu
Condition
Solution annealed; precipitation (age) hardened at 480°C; air cooled
UNS number
J92180
US name
ASTM CB-7Cu
ASTM CB-7Cu Typical uses
Aerospace, chemical processing, food processing, gas turbine, marine, petrochemical industry, pulp and paper industries
ASTM CB-7Cu Aged at 480°C Composition detail
C (carbon)
0
–
0.07
%
Cr (chromium)
15.5
–
17.7
%
Cu (copper)
2.5
–
3.2
%
Fe (iron)
72.3
–
78.2
%
Mn (manganese)
0
–
0.7
%
N (nitrogen)
0
–
0.05
%
Nb (niobium)
0.15
–
0.35
%
Ni (nickel)
3.6
–
4.6
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.03
%
Si (silicon)
0
–
1
%
ASTM CB-7Cu Physical properties
Density
7.7
–
7.8
g/cm3
ASTM CB-7Cu Aged at 480°C Mechanical properties
Young’s modulus
190
–
200
GPa
Specific stiffness
24.5
–
25.8
MN.m/kg
Yield strength (elastic limit)
1050
–
1170
MPa
Tensile strength
1160
–
1420
MPa
Specific strength
135
–
151
kN.m/kg
Elongation
7
–
13
% strain
Compressive strength
1050
–
1070
MPa
Flexural modulus
190
–
200
GPa
Flexural strength (modulus of rupture)
1050
–
1070
MPa
Shear modulus
73
–
79
GPa
Bulk modulus
140
–
156
GPa
Poisson’s ratio
0.275
–
0.285
Shape factor
20
Hardness – Vickers
402
–
422
HV
Hardness – Rockwell C
39
–
45
HRC
Hardness – Brinell
370
–
411
HB
Elastic stored energy (springs)
2830
–
3510
kJ/m3
Fatigue strength at 10^7 cycles
474
–
548
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
415
–
626
MPa
ASTM CB-7Cu Impact & fracture properties
Fracture toughness
30
–
44
MPa.m0.5
Toughness (G)
4.76
–
9.64
kJ/m2
ASTM CB-7Cu Aged at 480°C Thermal properties
Melting point
1490
–
1530
°C
Maximum service temperature
700
–
750
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
15
–
19
W/m.°C
Specific heat capacity
450
–
470
J/kg.°C
Thermal expansion coefficient
9.5
–
12.5
µstrain/°C
Thermal shock resistance
450
–
605
°C
Thermal distortion resistance
1.3
–
1.85
MW/m
Latent heat of fusion
260
–
285
kJ/kg
ASTM CB-7Cu Electrical properties
Electrical resistivity
72
–
82
µohm.cm
Electrical conductivity
2.1
–
2.39
%IACS
Galvanic potential
-0.19
–
-0.11
V
ASTM CB-7Cu Magnetic properties
Magnetic type
Magnetic
ASTM CB-7Cu Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
4950
–
5080
m/s
Mechanical loss coefficient (tan delta)
3.2e-4
–
3.9e-4
ASTM CB-7Cu Processing properties
Metal casting
Acceptable
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
11 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency
0.66 – 0.9
ASTM CB-7Cu Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aging martensitic steels at a low temperatures, around 480 °C, improves resistance. Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
ASTM CB-7Cu Aged at 480°C Corrosion resistance
Pitting resistance equivalent number (PREN)
15.5 – 18.5
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Not susceptible
ASTM CB-7Cu Notes
ASTM CB-7Cu Aged at 480°C Warning
Castings intended to be welded should have Cu content <3%, to avoid underbead cracking.
ASTM CB-7Cu Aged at 480°C Other notes
Lime-coated electrodes of similar composition should be used for welding by shielded metal-arc process.