15-5PH H900 Stainless Steel Material Data Sheet

15-5PH H900 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

15-5PH H900 Stainless Steel Overview

15-5PH H900 stainless steel is a martensitic precipitation hardening stainless steel (UNS S15500) in the wrought form. Condition: H900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled). This 15-5PH H900 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 15-5PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 15-5PH parts in-house and inspects them before shipment.

15-5PH Designation

15-5PH, wrought
ConditionH900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled)
UNS numberS15500
US name15-5PH

15-5PH Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

15-5PH H900 Stainless Steel Composition detail

C (carbon)0–0.07%
Cr (chromium)14–15.5%
Cu (copper)2.5–4.5%
Fe (iron)71.9–79.8%
Mn (manganese)0–1%
Nb (niobium)0.15–0.4%
Ni (nickel)3.5–5.5%
P (phosphorus)0–0.04%
S (sulfur)0–0.03%
Si (silicon)0–1%
Ta (tantalum)0–0.05%

15-5PH Physical properties

Density7.79–7.87g/cm3

15-5PH H900 Stainless Steel Mechanical properties

Young’s modulus197–207GPa
Specific stiffness25.1–26.5MN.m/kg
Yield strength (elastic limit)1170–1300MPa
Tensile strength1310–1450MPa
Specific strength150–165kN.m/kg
Elongation13–15.1% strain
Compressive strength986–1090MPa
Flexural modulus197–207GPa
Flexural strength (modulus of rupture)1170–1300MPa
Shear modulus77–80.9GPa
Bulk modulus142–150GPa
Poisson’s ratio0.27–0.281 
Shape factor19
Hardness – Vickers250–460HV
Hardness – Rockwell B113–116HRB
Hardness – Rockwell C42–47HRC
Hardness – Brinell398–442HB
Elastic stored energy (springs)3400–4160kJ/m3
Fatigue strength at 10^7 cycles364–542MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357–552MPa

15-5PH Impact & fracture properties

Fracture toughness79.7–97.4MPa.m0.5
Toughness (G)31.7–46.5kJ/m2

15-5PH H900 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature282–316°C
Minimum service temperature-73–-43°C
Thermal conductivity17.8–19.3W/m.°C
Specific heat capacity440–458J/kg.°C
Thermal expansion coefficient10.6–11.2µstrain/°C
Thermal shock resistance527–595°C
Thermal distortion resistance1.62–1.78MW/m
Latent heat of fusion260–285kJ/kg

15-5PH Electrical properties

Electrical resistivity72–82µohm.cm
Electrical conductivity2.1–2.39%IACS
Galvanic potential-0.22–-0.14V

15-5PH Magnetic properties

Magnetic typeMagnetic

15-5PH Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5010–5140m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

15-5PH Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed12.2 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.608 – 0.895

15-5PH Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aging martensitic steels at a low temperatures, around 480 °C, improves resistance. Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

15-5PH H900 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)14 – 15.5
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Slightly susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasRestricted

15-5PH Standards with similar compositions

China: 0Cr16Ni4Cu4Nb to GB 8732
France: Z6CNU15.05 to AFNOR NF A35-581
Germany: GX4CrNiCuNb16-4 to DIN
USA: 17-4PH to SAE J467, 5658 to AMS 5658, 5659 to AMS 5659, 5826 to AMS 5826, 5862 to AMS 5862, S15500 to ASTM A564/A564M, S15500 to ASTM A693, S15500 to ASTM A705/A705M-95, S15500 to ASTM A959, UNS J92110, UNS S15500