FV520 BS S144 is a martensitic precipitation hardening stainless steel (EN 1.4594) in the wrought form. Condition: Solution treated at 1000°C, primary hardened at 800°C, precipitation hardened at 450°C. This FV520 BS S144 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for FV520 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined FV520 parts in-house and inspects them before shipment.
FV520 Designation
FV520 (BS S144), wrought
Condition
Solution treated at 1000°C, primary hardened at 800°C, precipitation hardened at 450°C
EN name
X5CrNiMoCuNb14-5 to BS EN 10088-1, BS EN 10088-3, BS S 143, BS S 144, BS S 145
EN number
1.4594
Tradenames
Firth Vickers FV520, FV520B
FV520 Typical uses
Blading, bolts, fasteners, valves, pumps, water impellers, and assemblies, in the aviation and aerospace industries, nuclear, turbine and general mechanical engineering.
FV520 (BS S144) Composition detail
C (carbon)
0
–
0.07
%
Cr (chromium)
13.2
–
14.7
%
Cu (copper)
1.2
–
2
%
Fe (iron)
73.3
–
79.3
%
Mn (manganese)
0
–
1
%
Mo (molybdenum)
1.2
–
2
%
Nb (niobium)
0.1
–
0.4
%
Ni (nickel)
5
–
5.8
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.025
%
Si (silicon)
0
–
0.7
%
FV520 Physical properties
Density
7.82
–
7.83
g/cm3
FV520 (BS S144) Mechanical properties
Young’s modulus
206
–
216
GPa
Specific stiffness
26.3
–
27.6
MN.m/kg
Yield strength (elastic limit)
1030
–
1200
MPa
Tensile strength
1130
–
1330
MPa
Specific strength
132
–
153
kN.m/kg
Elongation
12
–
18
% strain
Compressive modulus
206
–
216
GPa
Compressive strength
1030
–
1200
MPa
Flexural modulus
206
–
216
GPa
Flexural strength (modulus of rupture)
924
–
1090
MPa
Shear modulus
78
–
82
GPa
Shear strength
756
–
882
MPa
Bulk modulus
172
–
180
GPa
Poisson’s ratio
0.295
–
0.305
Shape factor
21.9
Hardness – Vickers
370
–
420
HV
Hardness – Rockwell C
38
–
43
HRC
Hardness – Brinell
352
–
401
HB
Elastic stored energy (springs)
2520
–
3400
kJ/m3
Fatigue strength at 10^7 cycles
373
–
439
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
339
–
483
MPa
FV520 Impact & fracture properties
Fracture toughness
106
–
129
MPa.m0.5
Toughness (G)
53.7
–
78.3
kJ/m2
FV520 (BS S144) Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
382
–
427
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
16.5
–
17.9
W/m.°C
Specific heat capacity
471
–
490
J/kg.°C
Thermal expansion coefficient
11
–
11.5
µstrain/°C
Thermal shock resistance
432
–
509
°C
Thermal distortion resistance
1.46
–
1.6
MW/m
Latent heat of fusion
266
–
327
kJ/kg
FV520 Electrical properties
Electrical resistivity
80
–
85
µohm.cm
Electrical conductivity
2.03
–
2.16
%IACS
FV520 Magnetic properties
Magnetic type
Magnetic
FV520 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5130
–
5250
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
FV520 Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Unsuitable
Machining speed
10.4 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIG
Fair
Weldability – plasma
Good
Weldability – SAW
Fair
Weldability – TIG
Good
Brazeability
Good
Carbon equivalency
0.912 – 1.21
FV520 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Limited use
Flammability
Non-flammable
FV520 (BS S144) Corrosion resistance
Pitting resistance equivalent number (PREN)
17.9 – 20.8
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide