17-4PH Cast H1100 Stainless Steel Material Data Sheet

17-4PH Cast H1100 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

17-4PH Cast H1100 Overview

17-4PH cast H1100 is a martensitic precipitation hardening stainless steel (UNS S17400) in the cast form. Condition: H1100 – Solution treated and precipitation/age hardened at 1100°F (593°C). This 17-4PH cast H1100 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-4PH castings from Turkey (Türkiye)? Modulus Metal supplies 17-4PH castings with in-house CNC machining and inspects them before shipment.

17-4PH Designation

17-4PH
ConditionH1100 – Solution treated and precipitation/age hardened at 1100°F (593°C)
UNS numberS17400
US nameASTM S17400, ASTM 61, AMS 5355
GB (Chinese) name0Cr17Ni4Cu4Nb, 0Cr16Ni4Cu4Nb
JIS (Japanese) nameSUSF630, SUS630
Tradenames17-4 PH, AK Steel (USA); 17-4PH, Sandmeyer (USA); CATAMOLD 17-4PH, BASF (USA); AMS 5643 – 17/4 PH, Smiths (UK);

17-4PH Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

17-4PH Cast H1100 Composition detail

Al (aluminum)0–0.05%
C (carbon)0–0.06%
Cr (chromium)15.5–16.7%
Cu (copper)2.8–3.5%
Fe (iron)72.8–77.4%
Mn (manganese)0–0.7%
N (nitrogen)0–0.05%
Nb (niobium)0.15–0.4%
Ni (nickel)3.6–4.6%
P (phosphorus)0–0.025%
S (sulfur)0–0.025%
Si (silicon)0.5–1%
Sn (tin)0–0.02%
Ta (tantalum)0–0.05%

17-4PH Physical properties

Density7.82–7.9g/cm3

17-4PH Cast H1100 Mechanical properties

Young’s modulus197–207GPa
Specific stiffness25–26.4MN.m/kg
Yield strength (elastic limit)827–914MPa
Tensile strength896–990MPa
Specific strength105–116kN.m/kg
Elongation6–6.97% strain
Compressive strength910–1010MPa
Flexural modulus197–207GPa
Flexural strength (modulus of rupture)827–914MPa
Shear modulus88–92.5GPa
Bulk modulus142–150GPa
Poisson’s ratio0.27–0.281 
Shape factor27
Hardness – Vickers250–460HV
Elastic stored energy (springs)1690–2070kJ/m3
Fatigue strength at 10^7 cycles364–542MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357–552MPa

17-4PH Impact & fracture properties

Fracture toughness138–168MPa.m0.5
Toughness (G)94.6–139kJ/m2

17-4PH Cast H1100 Thermal properties

Melting point1400–1440°C
Maximum service temperature282–316°C
Minimum service temperature-73–-43°C
Thermal conductivity17.3–18.7W/m.°C
Specific heat capacity477–496J/kg.°C
Thermal expansion coefficient12.5–13.1µstrain/°C
Thermal shock resistance316–357°C
Thermal distortion resistance1.34–1.47MW/m
Latent heat of fusion260–285kJ/kg

17-4PH Electrical properties

Electrical resistivity75–85µohm.cm
Electrical conductivity2.03–2.3%IACS
Galvanic potential-0.2–-0.12V

17-4PH Magnetic properties

Magnetic typeMagnetic

17-4PH Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5000–5130m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

17-4PH Processing properties

Metal castingLimited use
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed14 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency0.687 – 0.867

17-4PH Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

17-4PH Cast H1100 Corrosion resistance

Pitting resistance equivalent number (PREN)15.5 – 17.5
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Slightly susceptible

17-4PH Standards with similar compositions

USA: 5342 to AMS 5342D, UNS J92150, UNS J92200
Tradenames: COOPER 17-4 PH, CORROSALLOY HT, ISO-CAST CB7CU, T-17-4PH, ZCR 173