15-5PH Cast H935 Stainless Steel Material Data Sheet
15-5PH Cast H935 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
15-5PH Cast H935 Overview
15-5PH cast H935 is a martensitic precipitation hardening stainless steel (UNS S15500) in the cast form. In the H935 condition it is solution annealed, then age hardened at 502°C and air cooled. This 15-5PH cast H935 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 15-5PH castings from Turkey (Türkiye)? Modulus Metal supplies 15-5PH castings with in-house CNC machining and inspects them before shipment.
15-5PH Designation
15-5PH
Condition
H935 (Solution annealed; precipitation (age) hardened at 502°C; air cooled)
UNS number
S15500
US name
15-5PH
15-5PH Cast H935 Composition detail
C (carbon)
0
–
0.05
%
Cr (chromium)
14
–
15.5
%
Cu (copper)
2.5
–
3.2
%
Fe (iron)
74.2
–
78.6
%
Mn (manganese)
0
–
0.6
%
N (nitrogen)
0
–
0.05
%
Nb (niobium)
0.15
–
0.3
%
Ni (nickel)
4.2
–
5
%
P (phosphorus)
0
–
0.025
%
S (sulfur)
0
–
0.025
%
Si (silicon)
0.5
–
1
%
Ta (tantalum)
0
–
0.05
%
15-5PH Physical properties
Density
7.77
–
7.84
g/cm3
15-5PH Cast H935 Mechanical properties
Young’s modulus
197
–
207
GPa
Specific stiffness
25.2
–
26.5
MN.m/kg
Yield strength (elastic limit)
1030
–
1140
MPa
Tensile strength
1170
–
1300
MPa
Specific strength
132
–
146
kN.m/kg
Elongation
6
–
6.97
% strain
Compressive strength
1070
–
1180
MPa
Flexural modulus
197
–
207
GPa
Flexural strength (modulus of rupture)
1030
–
1140
MPa
Shear modulus
77
–
80.9
GPa
Bulk modulus
142
–
150
GPa
Poisson’s ratio
0.27
–
0.281
Shape factor
21
Hardness – Vickers
250
–
460
HV
Elastic stored energy (springs)
2650
–
3230
kJ/m3
Fatigue strength at 10^7 cycles
364
–
542
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357
–
552
MPa
15-5PH Impact & fracture properties
Fracture toughness
83.7
–
102
MPa.m0.5
Toughness (G)
35
–
51.4
kJ/m2
15-5PH Cast H935 Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
282
–
316
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
18
–
19.5
W/m.°C
Specific heat capacity
440
–
458
J/kg.°C
Thermal expansion coefficient
12.5
–
13.1
µstrain/°C
Thermal shock resistance
395
–
446
°C
Thermal distortion resistance
1.39
–
1.53
MW/m
Latent heat of fusion
260
–
285
kJ/kg
15-5PH Electrical properties
Electrical resistivity
72
–
82
µohm.cm
Electrical conductivity
2.1
–
2.39
%IACS
Galvanic potential
-0.22
–
-0.14
V
15-5PH Magnetic properties
Magnetic type
Magnetic
15-5PH Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5020
–
5150
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
15-5PH Processing properties
Metal casting
Limited use
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
12.2 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency
0.637 – 0.81
15-5PH Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
15-5PH Cast H935 Corrosion resistance
Pitting resistance equivalent number (PREN)
14 – 16.3
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Not susceptible
15-5PH Standards with similar compositions
India: Grade 2 to IS 11758
USA: 5346 to AMS 5346B, 5347 to AMS 5347A, 5357 to AMS 5357A, CB7Cu-2 to ASTM A747/A747M