PPA 33% Glass Fiber Material Data Sheet

PPA 33% Glass Fiber (Polyphthalamide) Material Data Sheet

PPA 33% Glass Fiber Overview

PPA 33% glass fiber is a grade of polyphthalamide (PPA), designated Polyphthalamide (33% glass fiber). This PPA 33% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PPA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PPA parts in-house and inspects them before shipment.

PPA 33% Glass Fiber Designation

Polyphthalamide (33% glass fiber)
TradenamesAmodel, Edgetek, Grivory, Zytel

PPA 33% Glass Fiber Typical uses

Industrial and chemical processing equipment, bearings, gears, electrical connectors, packaging, under bonnet automobile applications

PPA 33% Glass Fiber Composition detail

Polymer67  %
Glass (fiber)33  %

PPA 33% Glass Fiber Physical properties

Density1.46–1.49g/cm3

PPA 33% Glass Fiber Mechanical properties

Young’s modulus10.9–13.6GPa
Specific stiffness7.39–9.22MN.m/kg
Yield strength (elastic limit)166–207MPa
Tensile strength168–205MPa
Specific strength113–140kN.m/kg
Elongation1.74–2.51% strain
Elongation at yield1.47–2.78% strain
Compressive modulus11.6–12.9GPa
Compressive strength212–235MPa
Flexural modulus10.1–12.1GPa
Flexural strength (modulus of rupture)223–273MPa
Shear modulus4.4–4.63GPa
Shear strength71.7–87.6MPa
Bulk modulus13.5–14.9GPa
Poisson’s ratio0.343–0.356 
Shape factor6.23
Hardness – Vickers53–59HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)1120–1780kJ/m3
Fatigue strength at 10^7 cycles70.8–78.2MPa

PPA 33% Glass Fiber Impact & fracture properties

Fracture toughness5.07–5.61MPa.m0.5
Toughness (G)2.02–2.7kJ/m2
Impact strength, notched 23 °C5.95–11.6kJ/m2
Impact strength, notched -30 °C5.51–12kJ/m2
Impact strength, unnotched 23 °C45.6–66.9kJ/m2
Impact strength, unnotched -30 °C44–66kJ/m2

PPA 33% Glass Fiber Thermal properties

Melting point299–322°C
Glass temperature119–135°C
Heat deflection temperature 0.45MPa284–340°C
Heat deflection temperature 1.8MPa258–313°C
Maximum service temperature215–235°C
Minimum service temperature-49–-29°C
Thermal conductivity0.458–0.474W/m.°C
Specific heat capacity1360–1410J/kg.°C
Thermal expansion coefficient23–58µstrain/°C
Thermal shock resistance259–671°C
Thermal distortion resistance0.00803–0.0203MW/m

PPA 33% Glass Fiber Electrical properties

Electrical resistivity1.55e18–3.87e19µohm.cm
Electrical conductivity4.46e-18–1.11e-16%IACS
Dielectric constant (relative permittivity)3.93–5.54 
Dissipation factor (dielectric loss tangent)0.00542–0.0143 
Dielectric strength (dielectric breakdown)25.3–43.2MV/m
Comparative tracking index575–600V

PPA 33% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PPA 33% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2710–3040m/s
Mechanical loss coefficient (tan delta)0.00754–0.00834 

PPA 33% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.2–0.33%
Water absorption @ sat3.3–4.4%
Humidity absorption @ sat1.4–2%

PPA 33% Glass Fiber Processing properties

Polymer injection moldingAcceptable
Polymer extrusionUnsuitable
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.5 %
Melt temperature268 – 349 °C
Molding pressure range34.4 – 103 MPa

PPA 33% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsLimited use
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsLimited use
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning