PA11 Rigid Grade (Polyamide 11) Material Data Sheet
PA11 Rigid Grade Overview
PA11 rigid grade is a grade of polyamide 11 (PA11, nylon 11), designated Polyamide (Nylon) (Type 11, rigid, molding and extrusion). This PA11 rigid grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA11 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA11 parts in-house and inspects them before shipment.
PA11 Rigid Grade Designation
Polyamide (Nylon) (Type 11, rigid, molding and extrusion)
Tradenames
Ashlene, Hifill, Lubricomp, Rilsan
PA11 Rigid Grade Typical uses
Hose for air, hydraulic fluid or petrol, gears, cams, tool handles, powder for coatings for metals.
PA11 Rigid Grade Composition detail
Polymer
100
%
PA11 Rigid Grade Physical properties
Density
1.02
–
1.04
g/cm3
PA11 Rigid Grade Mechanical properties
Young’s modulus
1.06
–
1.33
GPa
Specific stiffness
1.03
–
1.29
MN.m/kg
Yield strength (elastic limit)
35.4
–
44.1
MPa
Tensile strength
50
–
55
MPa
Specific strength
34.4
–
42.8
kN.m/kg
Elongation
280
–
320
% strain
Elongation at yield
8
–
15
% strain
Compressive modulus
1.14
–
1.25
GPa
Compressive strength
60
–
66
MPa
Flexural modulus
1.09
–
1.3
GPa
Flexural strength (modulus of rupture)
56.9
–
69.6
MPa
Shear modulus
0.409
–
0.43
GPa
Shear strength
26.8
–
32.8
MPa
Bulk modulus
2.46
–
2.72
GPa
Poisson’s ratio
0.406
–
0.423
Shape factor
4.1
Hardness – Vickers
11
–
13
HV
Hardness – Rockwell M
70
–
80
Hardness – Rockwell R
100
–
110
Hardness – Shore D
70
–
75
Elastic stored energy (springs)
521
–
829
kJ/m3
Fatigue strength at 10^7 cycles
20
–
22
MPa
PA11 Rigid Grade Impact & fracture properties
Fracture toughness
3.17
–
3.5
MPa.m0.5
Toughness (G)
8.07
–
10.8
kJ/m2
Impact strength, notched 23 °C
7.5
–
11
kJ/m2
Impact strength, notched -30 °C
2.1
–
2.7
kJ/m2
Impact strength, unnotched 23 °C
590
–
600
kJ/m2
Impact strength, unnotched -30 °C
590
–
600
kJ/m2
PA11 Rigid Grade Thermal properties
Melting point
180
–
190
°C
Glass temperature
36
–
48
°C
Heat deflection temperature 0.45MPa
129
–
170
°C
Heat deflection temperature 1.8MPa
40
–
52
°C
Maximum service temperature
80
–
110
°C
Minimum service temperature
-70
–
-55
°C
Thermal conductivity
0.19
–
0.29
W/m.°C
Specific heat capacity
1730
–
1770
J/kg.°C
Thermal expansion coefficient
176
–
184
µstrain/°C
Thermal shock resistance
158
–
216
°C
Thermal distortion resistance
0.00106
–
0.00161
MW/m
Latent heat of fusion
39
kJ/kg
PA11 Rigid Grade Electrical properties
Electrical resistivity
2e19
–
5e20
µohm.cm
Electrical conductivity
3.45e-19
–
8.62e-18
%IACS
Dielectric constant (relative permittivity)
4.2
–
5.92
Dissipation factor (dielectric loss tangent)
0.0473
–
0.125
Dielectric strength (dielectric breakdown)
25
–
35
MV/m
Comparative tracking index
600
V
PA11 Rigid Grade Magnetic properties
Magnetic type
Non-magnetic
PA11 Rigid Grade Optical, aesthetic and acoustic properties
Refractive index
1.51
–
1.53
Transparency
Translucent
Acoustic velocity
1010
–
1140
m/s
Mechanical loss coefficient (tan delta)
0.023
–
0.0254
PA11 Rigid Grade Absorption & permeability
Water absorption @ 24 hrs
0.68
–
1.1
%
Water absorption @ sat
1.6
–
2.2
%
Humidity absorption @ sat
0.68
–
0.92
%
Water vapor transmission
0.41
g.mm/m².day
Permeability (O2)
17
cm³.mm/m².day.atm
PA11 Rigid Grade Processing properties
Polymer injection molding
Excellent
Polymer extrusion
Acceptable
Polymer thermoforming
Limited use
Linear mold shrinkage
1 – 2 %
Melt temperature
199 – 246 °C
Mold temperature
40 – 60 °C
Molding pressure range
16 – 70 MPa
PA11 Rigid Grade Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Unacceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Acceptable
Oils and fuels
Acceptable
Oxidation at 500C
Unacceptable
UV radiation (sunlight)
Fair
Flammability
Slow-burning
PA11 Rigid Grade Notes
PA11 Rigid Grade Other notes
PA type 11 is not petroleum-based, but uses C11 derivatives of castor oil (a vegetable oil extracted from castor seeds) as its main chemical feedstock.