PA11 Flexible Grade (Polyamide 11) Material Data Sheet
PA11 Flexible Grade Overview
PA11 flexible grade is a grade of polyamide 11 (PA11, nylon 11), designated Polyamide (Nylon) (Type 11, flexible, molding & extrusion). This PA11 flexible grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA11 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA11 parts in-house and inspects them before shipment.
Hose for air, hydraulic fluid or petrol, gears, cams, tool handles, powder for coatings for metals.
PA11 Flexible Grade Composition detail
Polymer
87
–
93
%
Plasticizer/oil
7
–
13
%
PA11 Flexible Grade Physical properties
Density
1.04
–
1.05
g/cm3
PA11 Flexible Grade Mechanical properties
Young’s modulus
0.35
–
0.36
GPa
Specific stiffness
0.335
–
0.345
MN.m/kg
Yield strength (elastic limit)
25
–
27
MPa
Tensile strength
45
–
51
MPa
Specific strength
23.9
–
25.8
kN.m/kg
Elongation
360
–
430
% strain
Elongation at yield
32
–
42
% strain
Compressive modulus
0.35
–
0.36
GPa
Compressive strength
54
–
61.2
MPa
Flexural modulus
0.31
–
0.33
GPa
Flexural strength (modulus of rupture)
36.3
–
39.2
MPa
Shear modulus
0.124
–
0.126
GPa
Shear strength
27
–
30.6
MPa
Bulk modulus
0.621
–
0.779
GPa
Poisson’s ratio
0.406
–
0.423
Shape factor
3.1
Hardness – Vickers
8
–
9
HV
Hardness – Rockwell M
48
Hardness – Rockwell R
78
Hardness – Shore D
66
–
67
Elastic stored energy (springs)
881
–
1030
kJ/m3
Fatigue strength at 10^7 cycles
18
–
20.4
MPa
PA11 Flexible Grade Impact & fracture properties
Fracture toughness
2.6
–
2.62
MPa.m0.5
Toughness (G)
18.9
–
19.5
kJ/m2
Impact strength, notched 23 °C
590
–
600
kJ/m2
Impact strength, notched -30 °C
6
–
7
kJ/m2
Impact strength, unnotched 23 °C
590
–
600
kJ/m2
Impact strength, unnotched -30 °C
590
–
600
kJ/m2
PA11 Flexible Grade Thermal properties
Melting point
182
–
192
°C
Glass temperature
36
–
48
°C
Heat deflection temperature 0.45MPa
130
°C
Heat deflection temperature 1.8MPa
45
°C
Maximum service temperature
90
–
105
°C
Minimum service temperature
-60
–
-40
°C
Thermal conductivity
0.19
–
0.29
W/m.°C
Specific heat capacity
1730
–
1770
J/kg.°C
Thermal expansion coefficient
110
µstrain/°C
Thermal shock resistance
639
–
693
°C
Thermal distortion resistance
0.00173
–
0.00264
MW/m
Latent heat of fusion
39
kJ/kg
PA11 Flexible Grade Electrical properties
Electrical resistivity
1e17
µohm.cm
Electrical conductivity
1.72e-15 %IACS
Dielectric constant (relative permittivity)
4.2
–
5.92
Dissipation factor (dielectric loss tangent)
0.0473
–
0.125
Dielectric strength (dielectric breakdown)
23
MV/m
Comparative tracking index
600
V
PA11 Flexible Grade Magnetic properties
Magnetic type
Non-magnetic
PA11 Flexible Grade Optical, aesthetic and acoustic properties
Refractive index
1.51
–
1.53
Transparency
Translucent
Acoustic velocity
578
–
587
m/s
Mechanical loss coefficient (tan delta)
0.0461
–
0.0475
PA11 Flexible Grade Absorption & permeability
Water absorption @ 24 hrs
0.3
%
Water absorption @ sat
1.6
%
Humidity absorption @ sat
0.9
%
Water vapor transmission
0.35
g.mm/m².day
Permeability (O2)
15
cm³.mm/m².day.atm
PA11 Flexible Grade Processing properties
Polymer injection molding
Excellent
Polymer extrusion
Limited use
Polymer thermoforming
Limited use
Linear mold shrinkage
1 – 2 %
Melt temperature
260 – 270 °C
Mold temperature
50 °C
Molding pressure range
16 – 70 MPa
PA11 Flexible Grade Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Unacceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Acceptable
Oils and fuels
Acceptable
Oxidation at 500C
Unacceptable
UV radiation (sunlight)
Fair
Flammability
Slow-burning
PA11 Flexible Grade Notes
PA11 Flexible Grade Other notes
PA type 11 is not petroleum-based, but uses C11 derivatives of castor oil (a vegetable oil extracted from castor seeds) as its main chemical feedstock.