Home » High Conductivity Copper » Cu-Cd-Sn H.C. Copper, Soft Material Data Sheet
Cu-Cd-Sn H.C. Copper Material Data Sheet (Wrought, Soft)
Cu-Cd-Sn Soft Copper Overview
Cu-Cd-Sn soft copper is a wrought high conductivity copper, known as h.c. copper. Condition: Soft. This Cu-Cd-Sn soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Cu-Cd-Sn copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Cu-Cd-Sn copper parts in-house and inspects them before shipment.
Cu-Cd-Sn Designation
Wrought Copper Alloy: hc-CuCd1Sn(s) Condition Soft UNS number C16400, C16500
Cu-Cd-Sn Typical uses
Catenary trolley wires, telephone wires, spring contacts, flexible cords, plugs & sockets, overhead lines.
Cu-Cd-Sn Soft Copper Composition detail
Cd (cadmium) 0.5 – 1 % Cu (copper) 98.4 – 99.3 % Sn (tin) 0.2 – 0.6 %
Cu-Cd-Sn Physical properties
Cu-Cd-Sn Soft Copper Mechanical properties
Young’s modulus 133 – 135 GPa Specific stiffness 14.9 – 15.1 MN.m/kg Yield strength (elastic limit) 85 – 95 MPa Tensile strength 250 – 280 MPa Specific strength 9.51 – 10.6 kN.m/kg Elongation 40 – 45 % strain Compressive strength 85 – 95 MPa Flexural modulus 133 – 135 GPa Flexural strength (modulus of rupture) 85 – 95 MPa Shear modulus 48 – 50 GPa Bulk modulus 144 – 146 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 30 Hardness – Vickers 57 – 59 HV Elastic stored energy (springs) 27 – 33.6 kJ/m3 Fatigue strength at 10^7 cycles 130 – 140 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 120 – 152 MPa
Cu-Cd-Sn Impact & fracture properties
Fracture toughness 77.6 – 80.9 MPa.m0.5 Toughness (G) 44.9 – 48.9 kJ/m2
Cu-Cd-Sn Soft Copper Thermal properties
Melting point 1010 – 1080 °C Maximum service temperature 77 – 87 °C Minimum service temperature -273 °C Thermal conductivity 207 – 248 W/m.°C Specific heat capacity 372 – 385 J/kg.°C Thermal expansion coefficient 17 – 17.5 µstrain/°C Thermal shock resistance 36.7 – 41.2 °C Thermal distortion resistance 12 – 14.4 MW/m Latent heat of fusion 200 – 208 kJ/kg
Cu-Cd-Sn Electrical properties
Electrical resistivity 2.29 – 2.88 µohm.cm Electrical conductivity 59.9 – 75.3 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.21 – -0.13 V
Cu-Cd-Sn Magnetic properties
Magnetic type Non-magnetic
Cu-Cd-Sn Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3860 – 3890 m/s Mechanical loss coefficient (tan delta) 4.43e-4 – 5.54e-4
Cu-Cd-Sn Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Acceptable Metal press forming Excellent Metal deep drawing Limited use Machining speed 29 m/min Weldability Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements Good
Cu-Cd-Sn Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
Cu-Cd-Sn Soft Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
Cu-Cd-Sn Notes
Cu-Cd-Sn Soft Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
Cu-Cd-Sn Standards with similar compositions
Germany: 2.127 to DIN, CuCdSn to DINUSA: C16500, UNS C16400, UNS C16500Tradenames: HITENSO 165, PHONO CADMIUM 955