Home » High Conductivity Copper » C16200 H.C. Copper, Soft Material Data Sheet
C16200 H.C. Copper Material Data Sheet (Wrought, Soft)
C16200 Soft Copper Overview
C16200 soft copper is a wrought high conductivity copper (UNS C16200, EN CW131C), known as h.c. copper. Condition: Soft. This C16200 soft copper material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C16200 copper parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined C16200 copper parts in-house and inspects them before shipment.
C16200 Designation
Wrought Copper Alloy: hc-CuCd1(s); C108 (UNS C16200) Condition Soft UNS number C16200 EN name CW131C ISO name CuCd1 GB (Chinese) name QCd1
C16200 Typical uses
Catenary trolley wires, telephone wires, spring contacts, flexible cords, plugs & sockets, overhead lines.
C16200 Soft Copper Composition detail
Cd (cadmium) 0.7 – 1.2 % Cu (copper) 98.8 – 99.3 % Fe (iron) 0 – 0.02 %
C16200 Physical properties
C16200 Soft Copper Mechanical properties
Young’s modulus 133 – 135 GPa Specific stiffness 14.9 – 15.1 MN.m/kg Yield strength (elastic limit) 80 – 90 MPa Tensile strength 250 – 270 MPa Specific strength 8.95 – 10.1 kN.m/kg Elongation 40 – 45 % strain Compressive strength 80 – 90 MPa Flexural modulus 133 – 135 GPa Flexural strength (modulus of rupture) 80 – 90 MPa Shear modulus 48 – 50 GPa Bulk modulus 144 – 146 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 30 Hardness – Vickers 58 – 60 HV Elastic stored energy (springs) 24 – 30.1 kJ/m3 Fatigue strength at 10^7 cycles 90 – 110 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 87.8 – 113 MPa
C16200 Impact & fracture properties
Fracture toughness 79.2 – 82.6 MPa.m0.5 Toughness (G) 46.8 – 50.9 kJ/m2
C16200 Soft Copper Thermal properties
Melting point 1010 – 1080 °C Maximum service temperature 77 – 87 °C Minimum service temperature -273 °C Thermal conductivity 310 – 351 W/m.°C Specific heat capacity 372 – 385 J/kg.°C Thermal expansion coefficient 16.8 – 16.9 µstrain/°C Thermal shock resistance 35.4 – 39.9 °C Thermal distortion resistance 18.4 – 20.8 MW/m Latent heat of fusion 200 – 208 kJ/kg
C16200 Electrical properties
Electrical resistivity 1.91 – 2.19 µohm.cm Electrical conductivity 78.7 – 90.3 %IACS Temperature dependence of resistivity 5.2 – 5.4 /°C Galvanic potential -0.2 – -0.12 V
C16200 Magnetic properties
Magnetic type Non-magnetic
C16200 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3860 – 3890 m/s Mechanical loss coefficient (tan delta) 4.94e-4 – 6.25e-4
C16200 Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Acceptable Metal press forming Excellent Metal deep drawing Limited use Machining speed 29.6 m/min Weldability Notes: Preheating and post weld heat treatment are not required, and contains hazardous elements Good
C16200 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
C16200 Soft Copper Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Not susceptible
C16200 Notes
C16200 Soft Copper Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
C16200 Standards with similar compositions
Australia: 162 to AS 1567, C16200 to AS 2738Czech Republic: CuCd1 to CSN 423058Germany: 2.1266 to DIN, CuCd1 to DINInternational: CuCd1 to ISO 1637, CuCd1 to ISO 1638, CuCd1 to ISO R1336Japan: CuCd1 to JIS Z3234Sweden: 5055-25 to SIS 145055UK: C108 to BS 2873, C108 to BS 2875USA: C16200, UNS C16200, UNS C16210Tradenames: ANSONIA ALLOY C 16200, BOLTOMET 210, BRIDGEPORT NO. 980, BRIDGEPORT NO. 985, BRONZE AU-CADMIUM, CADMIUM COPPER, CADMIUM COPPER 985, ELECTRAL CD 1, HITENSO 162, HI-TENSO 1622, LITHIUM-CONDUCTIVITY BRONZE, PHONO HI CONDUCTIVITY, PHONO HI-CONDUCTIVITY 985, TRIANGLE 80, TRIANGLE 85
Modulus Metal Services
Manufacturing & Quality Services in Turkey